Abstracts
A series of KF/γ-Al2O3 solid base catalysts were prepared by a wet impregnation method and applied to the synthesis of glycerol carbonate (GC) from glycerol and dimethyl carbonate. The influences of KF loading and calcination temperature of catalyst on the synthesis were investigated. The results showed that KF/γ-Al2O3 catalysts could promote glycerol conversion to GC efficiently. The structure and properties of the catalysts were studied by means of X-ray diffraction (XRD), Fourier transform infrared spectroscopy (FT-IR), N2-adsorption, CO2-temperature programmed desorption (TPD), X-ray photoelectron spectroscopy (XPS) and Hammett indicator method. It was found that several types of basic centers such as KF, KAlO2, KOH and possibly coordinately unsaturated F- ion existed on the catalysts. The strong basic centers could not only accelerate the conversion of glycerol, but also enhance the formation of glycidol from the decomposition of GC. The recycling of KF/γ-Al2O3 revealed that deactivation of catalyst was strengthened with the reuse times, which was mainly caused by the partial leaching of active potassium species. High calcination temperature favored the transformation of KF to KAlO2 and alleviated the deactivation of the catalyst. Based on the product distribution and obtained results, a possible reaction mechanism on reaction of glycerol with dimethyl carbonate was proposed.
glycerol; dimethyl carbonate; glycerol carbonate; KF/γ-A1(2)O3
Uma série de catalisadores sólidos básicos de KF/γ-Al2O3foi preparada pelo método deimpregnação úmida e aplicada à síntese de carbonato de glicerina (GC) a partir de glicerol e carbonato de dimetila. As influências do teor de KF e da temperatura de calcinação do catalisador na síntese foram investigadas. Os resultados mostraram que os catalisadores de KF/γ-Al2O3conseguem promover uma conversão eficiente de glicerol emGC. A estrutura e as propriedades dos catalisadores foram estudadas por difratometria de raios X (XRD), espectroscopia no infravermelho por transformada de Fourier (FTIR), adsorção de N2, dessorção térmica programada (TPD) de CO2, espectroscopia fotoeletrônica por raios X (XPS) e pelo método dos indicadores de Hammett. Observou-se que os catalisadores possuem vários tipos de centros básicos, como KF, KAlO2, KOH e possivelmente o íon F-coordenativamenteinsaturado. Os centros fortemente básicos não somente poderiam acelerar a conversão do glicerol, como também aumentar a formação do glicidol a partir da decomposição de GC. A reutilização de KF/γ-Al2O3 mostrou que a decomposição do catalisador, que é causada principalmente pela lixiviação parcial das espécies ativas de potássio, aumenta com o número de usos. Temperaturas altas de calcinação favorecem a transformação de KF emKAlO2e amenizam a desativação do catalisador. Com base na distribuição dos produtos e nos resultados obtidos, foi proposto um mecanismo possível para a reação do glicerol com carbonato de dimetila.
ARTICLE
Synthesis of glycerol carbonate by transesterification of glycerol and dimethyl carbonate over KF/ γ -Al2O3 catalyst
Zhenmin LiuI,II,III; Junwei WangI,* * e-mail: wangjw@sxicc.ac.cn ; Maoqing KangI; Ning YinI; Xinkui WangI; Yisheng TanII; Yulei ZhuII
ILaboratory of Applied Catalysis and Green Chemical Engineering
IIState Key Laboratory of Coal Conversion, Institute of Coal Chemistry, Chinese Academy of Sciences, 030001 Taiyuan, P. R. China
IIIUniversity of Chinese Academy of Sciences, 100049 Beijing, P. R. China
ABSTRACT
A series of KF/γ-Al2O3 solid base catalysts were prepared by a wet impregnation method and applied to the synthesis of glycerol carbonate (GC) from glycerol and dimethyl carbonate. The influences of KF loading and calcination temperature of catalyst on the synthesis were investigated. The results showed that KF/γ-Al2O3 catalysts could promote glycerol conversion to GC efficiently. The structure and properties of the catalysts were studied by means of X-ray diffraction (XRD), Fourier transform infrared spectroscopy (FT-IR), N2-adsorption, CO2-temperature programmed desorption (TPD), X-ray photoelectron spectroscopy (XPS) and Hammett indicator method. It was found that several types of basic centers such as KF, KAlO2, KOH and possibly coordinately unsaturated F- ion existed on the catalysts. The strong basic centers could not only accelerate the conversion of glycerol, but also enhance the formation of glycidol from the decomposition of GC. The recycling of KF/γ-Al2O3 revealed that deactivation of catalyst was strengthened with the reuse times, which was mainly caused by the partial leaching of active potassium species. High calcination temperature favored the transformation of KF to KAlO2 and alleviated the deactivation of the catalyst. Based on the product distribution and obtained results, a possible reaction mechanism on reaction of glycerol with dimethyl carbonate was proposed.
Keywords: glycerol, dimethyl carbonate, glycerol carbonate, KF/γ-A12O3
RESUMO
Uma série de catalisadores sólidos básicos de KF/γ-Al2O3foi preparada pelo método deimpregnação úmida e aplicada à síntese de carbonato de glicerina (GC) a partir de glicerol e carbonato de dimetila. As influências do teor de KF e da temperatura de calcinação do catalisador na síntese foram investigadas. Os resultados mostraram que os catalisadores de KF/γ-Al2O3conseguem promover uma conversão eficiente de glicerol emGC. A estrutura e as propriedades dos catalisadores foram estudadas por difratometria de raios X (XRD), espectroscopia no infravermelho por transformada de Fourier (FTIR), adsorção de N2, dessorção térmica programada (TPD) de CO2, espectroscopia fotoeletrônica por raios X (XPS) e pelo método dos indicadores de Hammett. Observou-se que os catalisadores possuem vários tipos de centros básicos, como KF, KAlO2, KOH e possivelmente o íon F-coordenativamenteinsaturado. Os centros fortemente básicos não somente poderiam acelerar a conversão do glicerol, como também aumentar a formação do glicidol a partir da decomposição de GC. A reutilização de KF/γ-Al2O3 mostrou que a decomposição do catalisador, que é causada principalmente pela lixiviação parcial das espécies ativas de potássio, aumenta com o número de usos. Temperaturas altas de calcinação favorecem a transformação de KF emKAlO2e amenizam a desativação do catalisador. Com base na distribuição dos produtos e nos resultados obtidos, foi proposto um mecanismo possível para a reação do glicerol com carbonato de dimetila.
Introduction
Biodiesel has attracted considerable attention as an alternative to the fossil fuel resources. European Union and U.S. government have promulgated mandatory regulations for the use of biodiesel in transportation fuel and on-road diesel.1 However, production of biodiesel by plant oil methanolysis generates large amount of glycerol (about 10 wt.%) as an unavoidable by-product, which has to be valorized to improve the economic competitiveness of biodiesel.2 Therefore, transformation of glycerol into value-added products is of great significance. So far, several routes for glycerol conversion have been reported, such as selective oxidation, reduction, etherification, esterification, polymerization, transesterification, etc.3,4
Among the various downstream products of glycerol, glycerol carbonate (4-hydroxymethyl-2-oxo-1,3-dioxolane, GC) represents an important and potential glycerol derivative that shows low toxicity and volatility, biodegradability, high boiling point, etc.5 GC has been widely used as a solvent in the cosmetics industry, as a membrane component for gas separation, as a component of coatings and detergents, as a precursor of glycidol, and as a monomer in preparing polycarbonate and polyurethane.6-8
GC can be synthesized from glycerol and different reagents including CO, CO2, phosgene, urea and organic carbonates. Among these raw materials, CO or phosgene is practically limited due to their toxicity and safety issues at both laboratory and industrial scales.9-11 The direct carbonation of glycerol with CO2 is thermodynamically limited and only gives very low yield even under harsh reaction conditions.12,13 The disadvantages of preparing GC from glycerol and urea lead to the creation of large amounts of ammonia and the difficulty in separating the undesired by-products like isocyanic acid and biuret.14,15 Although GC may be obtained from glycerol and ethylene carbonate by transesterification, ethylene glycol is produced as by-product which makes the separation of products difficult because of their high boiling points.16 Compared with these ways, transesterification of glycerol with dimethyl carbonate (DMC) for GC preparation is considered as the promising approach for industrial application due to the mild reaction conditions, easy separation, simple process and high GC yield.17-19
Several catalysts have been employed to promote this reaction efficiently. Kim et al.20 prepared GC in the presence of a lipase catalyst Novozym 435. However, the process is plagued by long reaction time, inconvenient removal of THF solvent and the sensitivity of lipase to environment. Recently, some homogeneous catalysts have been reported, they are tetra-N-butylammonium bromide, K2CO3, NaOH, etc.8,16,21,22 In spite of the high catalytic activity, these catalysts are less preferable in view of difficulty in separation of the spent catalyst from the reaction mixture and their poor reusability. To meet the requirement of future commercial production, development of efficient heterogeneous and recyclable catalyst is thus highly desirable. Ochoa-Gómez et al.16 found that the basic catalysts were more active than the acidic ones, and their catalytic activity depended on the basic strength and basicity of catalysts. Among the evaluated catalysts, CaO was found to be the best basic catalyst and gave 95% of GC yield. However, CaO was easily deactivated after adsorbing trace amount of water or CO2. Alvarez et al.18 prepared a series of Mg/Al mixed oxides from hydrotalcite and applied to the synthesis of GC as a solid base catalyst. 97% of glycerol conversion and 93% of GC yield were obtained under the optimized conditions. Takagaki et al.23 stated that the uncalcined hydrotalcite with hydromagnesite phase could also promote GC formation.
A number of reports have shown that the basic catalysts can accelerate the transesterification reaction efficiently. Besides CaO and hydrotalcite-like catalysts, alumina loaded KF also possesses strong basic sites, which can be prepared by simple impregnation and has been applied to various base-catalyzed reactions such as elimination, addition, condensation, epoxidation, transesterification, etc.24-26 So far, there are few reports concerning the application of KF/γ-Al2O3 as a solid base catalyst for the synthesis of GC from glycerol and DMC. Moreover, few reports discussed the effect of basic strength on the activity and selectivity of the catalyst in this process.
In this work, a series of KF/γ-Al2O3 catalysts were prepared by an impregnation method and used to the synthesis of GC from glycerol and DMC. The catalytic activities, surface properties and the reusability of catalysts were studied.
Experimental
Materials
Glycerol, KF and biphenyl were purchased from Tianjin Tianli Chemical Reagent Co., Ltd. DMC was obtained from Tangshan Chaoyang Chemical Engineering Co., Ltd. Glycidol (95%) and GC (90%) for gas chromatography analysis were purchased from Tianjin Kermel Chemical Reagent Co., Ltd. and TCI (Shanghai) Development Co. Ltd., respectively. DMC was distilled before use. All other reagents were used directly as received.
Catalyst preparation
The KF/γ-Al2O3 catalysts were prepared by a wet impregnation method. In a typical process, 0.4266 g, 0.9005 g, 1.4301 g, 3.4730 g and 6.6301 g of KF2H2O were separately dissolved in 7.5 mL of distilled water to obtain several KF solutions. 5 g of γ-Al2O3 was added into the above KF solutions, respectively. The mixture was stirred at room temperature for 10 min and dried at 110 ºC for 12 h. The obtained samples were calcined at 100-800 ºC for 5 h. Finally, the solids were crushed into particles for use as catalyst.
Catalyst characterization
X-ray diffraction (XRD) was measured on a Siemens D8 advance powder X-ray diffractometer using Ni-filtered Cu Kα radiation over a 2θ range of 5-80º with a step size of 0.02º at a scanning speed of 2º min-1.
Fourier transform infrared spectroscopy (FT-IR) data were collected on a Nicolet 380 FTIR instrument over the scanning range of 400-4000 cm-1 at a resolution of 4.0 cm-1. The catalyst sample was diluted with KBr at the ratio of 1:200 and pressed into a disk.
The surface basic properties of the catalysts were measured by CO2 temperature programmed desorption (TPD) using a TPD flow system equipped with a TCD detector (CHEMBET-3000 TPR/TPD, Quantachrome Instruments, USA). Experiments were carried out in the temperature range of 40-500 ºC. Before TPD experiments, the samples (about 100 mg) were pretreated at 350 ºC in a flow of nitrogen (20 mL min-1). The particle size of the catalyst was in the range of 40-60 mesh.
The basic strength and basicity of the solid catalysts were determined by the Hammett indicator. About 100 mg of the catalyst was ultrasonicated in 5 mL cyclohexane containing Hammett indicator and then the catalyst was left still for one hour to achieve equilibration. The basicity (expressed in mmol g-1) of the catalysts was measured using Hammett indicator-benzene carboxylic acid (0.05 mol L-1 anhydrous cyclohexane solution) titration. In typical experiment, the following Hammett indicators were used: bromothymol blue (H_=7.2), phenolphthalein (H_=9.8), 2,4-dinitroaniline (H_=15.0) and 4-nitroaniline (H_=18.4).
The surface area and pore volume of the catalyst were measured by nitrogen adsorption at 77.3 K on a Tristar 3000 surface area and porosity analyzer (USA). High purity nitrogen (99.99%) was used in this analysis. Prior to the measurement, the catalysts were outgassed at 200 ºC for 2 h under vacuum.
X-ray photoelectron spectroscopy (XPS) was used to measure the elemental composition on the catalyst surface and the data were collected on an XSAM800 spectrometer (KRATOS). Al Kα radiation (hν = 1486.6 eV) was used as the X-ray source.
Catalytic reaction
For this transesterification reaction, glycerol (18.40 g, 0.2 mol), DMC (54.0 g, 0.6 mol) and the catalyst (4 wt.% of glycerol) were added into a three-neck round-bottom flask equipped with a mechanical stirring bar, a thermometer and a condenser connected to a liquid dividing head for separating the formed methanol. The mixture was heated to 80 ºC and kept for 1.5 h under stirring. After reaction, the mixture was filtered to remove the catalyst. The liquid solution was distillated at 50 ºC under reduced pressure to remove methanol and DMC.
Procedure for recycling the catalyst
After reaction, the filtered catalysts were washed twice with 100 mL methanol, dried at 110 ºC for 2 h and then collected for the next run.
Product analysis
The product was analyzed on a gas chromatograph (GC-2014 Shimadzu, Japan) with a CBP-20 capillary column (25 m × 0.25 mm × 0.25 µm) and a flame ionization detector. The capillary column temperature was started at 75 ºC and maintained for 5 min, then raised at a rate of 30 ºC min-1 up to 240 ºC and maintained for 30 min. The detector and injection temperature were kept at 280 ºC and 250 ºC, respectively. Nitrogen was used as the carrier gas. Biphenyl was chosen as the internal standard for the quantitative analysis of products.
Results and Discussion
Catalyst characterization
For the KF/γ-Al2O3 catalyst, solid state reactions between KF and γ-Al2O3 occurred during the calcination process and several new phases such as K3AlF6, KOH, KAlO2 and [Al-OH···F-] might be formed.25 The new phases might constitute the strong basic centers and provided the catalytic activity for the transesterification. To find out the actual active phases, XRD was used to learn the structure of KF/γ-Al2O3 catalysts with various KF loading. The patterns are shown in Figure 1. The diffraction peaks of γ-Al2O3 (Figure 1a) were in good agreement with the International Centre for Diffraction Data powder diffraction file (PDF) 29-0063. When 5 wt.% of KF was loaded on γ-Al2O3, the catalyst displayed similar XRD patterns (Figure 1b) to that of γ-Al2O3, indicating that KF or its derivatives were highly dispersed on the surface of the support, or their amounts was smaller than those detectable via the XRD technique. When the KF loading rose up to 15 wt.%, the diffraction peaks at 2θ = 29.8º, 36.7º, 42.8º, 53.2º and 62.3º attributed to K3AlF6 (PDF 03-0615) were observed in Figure 1c. Meanwhile, the weak peaks of KAlO2 (PDF 53-0809) appeared at 2θ = 32.7º, 35.9º, 38.6º, 46.9º and 58.5º. The characteristic peaks of K3AlF6 and KAlO2 were strengthened gradually with further increasing KF loading, as illustrated in Figure 1d. In the XRD pattern (Figure 1e) of 45 wt.% KF/γ-Al2O3, a new diffraction peak appearing at 2θ = 30.9º was ascribed to KOH, as supported by reference.27
As reported, the formation of KOH was inevitable in company with K3AlF6.28 However, no peaks related to KOH were observed in XRD pattern of the 15 wt.% KF/γ-Al2O3, whereas peaks of KAlO2 began to appear. When the KF loading increased up to 45 wt.%, the characteristic peak of KOH appeared, meanwhile, the peak intensity of γ-Al2O3 decreased gradually, representing that the formed KOH reacted with γ-Al2O3 and was converted to KAlO2. This also indicated that the redundant KOH was accumulated on the catalyst surface and was detected by XRD. Thus, it was inferred that KAlO2 resulted from the interaction of KOH with γ-Al2O3. These results clearly showed that the loaded KF reacted with γ-Al2O3 and formed various new phases.
Additionally, the decrease of peak intensity of γ-Al2O3 also indicated that its crystal structure was destroyed through the solid-state reaction between KF and γ-Al2O3. Accordingly, the surface area and pore volume decreased and the pore size of catalyst increased with the KF loading. These data are tabulated in Table 1.
Figure 2 gives the FT-IR spectra of γ-Al2O3 and KF/γ-Al2O3 catalysts. As shown in Figure 2a, the characteristic bands at 3500 cm-1 and 1633 cm-1 were attributed to the stretching vibration and bending vibration of the OH group on γ-Al2O3, respectively. The band at 1073 cm-1 was assigned to Al-O-Al symmetric stretching vibrations. The bands appearing between 520 and 750 cm-1 was related to the vibrations of Al-O bonds corresponding to aluminum ions in octahedral and tetrahedral environments.29 Their band intensity decreased and even disappeared with the increasing KF loading, indicating that γ-Al2O3 reacted with KF. At the same process, a new peak at 586 cm-1 appeared which belonged to the Al-F stretching vibration in K3AlF6.26 The peak at 3500 cm-1 in Figure 2b-d was related to the stretching vibration of the Al-O-K group in KAlO2 and became broader with increasing KF loading.30 Qiu et al.27 proved that even the pure KOH showed a weak band at 3502 cm-1. Thus, the adsorption peak at about 3500 cm-1 was mainly ascribed to KAlO2. The FT-IR data further confirmed the formation of K3AlF6, KOH and KAlO2 in the solid interaction of KF and Al2O3.
CO2 temperature programmed desorption was utilized to study the basic properties of KF/γ-Al2O3 catalysts. The CO2-TPD curves of KF/γ-Al2O3 catalysts with different KF loading are shown in Figure 3. Three desorption peaks appeared in CO2-TPD curves at about 225, 340 and 490-580 ºC. They represented the weak, medium and strong basic centers of the KF/γ-Al2O3 catalyst, respectively. It was found from the desorption peak area in Figure 3a-c that the number of the strong basic centers of the KF/γ-Al2O3 catalyst increased markedly with the KF loading up to 15 wt.%. This could be ascribed to the formation of much more strong basic centers which were regarded as the active centers for the transesterification reaction.31,32 However, the basic sites (shown in Figure 3d-e) of KF/γ-Al2O3 catalysts were reduced gradually with the further increase of KF loading. The XRD patterns had indicated that K3AlF6 was easily formed and aggregated at high KF loading. Hence, the decrease of strong basic sites for KF/γ-Al2O3 catalysts at high KF loading might be attributed to the coverage by K3AlF6 and the structure damage resulting from the reaction between KF and γ-Al2O3.
The basic strength and basicity of the KF/γ-Al2O3 catalysts were measured quantitatively using Hammett indicators. The results are shown in Table 2. The carrier γ-Al2O3 was amphoteric and could not change the color of bromothymol blue (H_ = 7.2). Its basic strength were improved by impregnating KF and accordingly the color of phenolphthalein (H_ = 9.8) could be changed from white to red. However, all the KF/γ-Al2O3 catalysts could not change the color of 2,4-dinitroaniline (H_ = 15.0). This indicated that the basic strength of KF/γ-Al2O3 catalysts was in the range of 9.8-15.0 and the catalyst could be regarded as strong base according to Tanabe's definition.33 Moreover, the basicity of γ-Al2O3 was enhanced by impregnating KF and the maximum 0.298 mmol g-1 was taken when 15 wt.% KF was loaded. Exorbitant KF loading would reduce the basicity of catalyst, probably caused by the coverage of the conglomerated K3AlF6 and the reduction of surface area of the catalysts. The results well corresponded with the CO2-TPD characterization and the similar phenomenon was reported in references.34,35
Synthesis of GC from glycerol and DMC catalyzed by KF/γ-Al2O3
From Table 3, it was seen that γ-Al2O3 could not promote the transformation of glycerol into GC. KF·2H2O had unsatisfied activity for GC formation, and 48.7% of glycerol conversion was obtained after reacting at 80 ºC for 1.5 h. However, above 99% of glycerol conversion was gained under the same reaction conditions as GC synthesis when KF·2H2O was calcined at 400 ºC for 3 h. Since glycerol is strongly hydrophilic, adsorbing trace amount of water from environment is unavoidable. Ando et al.25 found that water played an important role in determining the activity of the catalyst. They believed that an active basic site involving a coordinately unsaturated F- ion [Al-OH···F-] was formed through the strong H-bond interaction. Zhu et al.36 also reported that neutral KF adsorbed trace amount of water vapor and formed a similar basic site. Obviously, the high activity of KF for glycerol conversion was related to the formation of a coordinately unsaturated F- ion through adsorbing trace amount of water. As to the lower activity of KF·2H2O, long time was taken to lose crystal water and then produced coordinately unsaturated F- ion. Thus, it was reasonable to obtain lower catalytic activity of KF·2H2O than that of KF.
Table 3 shows the catalytic performance of KF/γ-Al2O3 catalysts. It was found that glycerol conversion and GC yield markedly increased by introducing KF onto γ-Al2O3. As described in Table 2, the basic strength of γ-Al2O3 increased after KF loading. Accordingly, the catalytic activity was improved greatly, indicating that the high basic strength facilitated the conversion of glycerol. As KF loading was increased up to 15 wt.%, the catalytic activities and selectivity of KF/γ-Al2O3 catalysts increased. They possessed the same basic strength and the increased basicity with KF loading increased, presenting that the basicity favored the glycerol conversion at the given basic strength.
However, further elevating KF loading only resulted in the loss of GC selectivity. In the previous XRD characterization, it had been indicated that the amount of strong basic sites such as KAlO2, KOH increased with the KF loading. In the catalytic performance, pure KOH with the basic strength above 18.4 gave a total glycerol conversion and 42.5% of selectivity to glycidol which was produced from the decomposition of GC. Therefore, it was clearly inferred that too much strong basic sites on the catalyst promoted the decomposition of GC to glycidol. Bai et al.19 also stated that the too strong base led to the generation of glycidol.
The influence of calcination temperature on catalytic activity of KF/γ-Al2O3 was also investigated. The results are displayed in Table 3. No obvious changes for glycerol conversion and GC selectivity were observed for 15 wt.% KF/γ-Al2O3 catalysts calcined at 100 ºC and 400 ºC, respectively. Compared with those, KF/γ-Al2O3 calcined at 600 ºC showed lower activity, probably due to the transformation of active species at elevated temperature, although their XRD patterns (shown in Figure 4a-b and Figure 1c) were similar. Thus, it was deduced that [Al-OH···F-] phase might act an important role in glycerol conversion, especially at the low calcination temperature. With the calcination temperature increased, [Al-OH···F-] phase was destroyed and new basic phases such as KOH, KAlO2 were formed and provided new active basic sites to promote the conversion of glycerol. However, at the higher temperatures, excessive dehydroxyl, structure collapse and the formation of inactive AlF3 would weaken the activity of the catalyst seriously. Accordingly, inactive AlF3 (PDF 44-0231) was detected in XRD pattern (Figure 4c) of 15 wt.% KF/γ-Al2O3 catalyst calcined at 800 ºC. Ando et al.25 and Zhu et al.36 reported the solid state reactions occurred at various temperatures for KF/γ-Al2O3 catalyst and the [Al-OH···F-] structure, KOH, KAlO2, K3AlF6 and AlF3 were found.
The characterization and catalytic performance of KF/γ-Al2O3 have indicated that various basic sites existed on the surface of KF/γ-Al2O3 catalyst. To learn the effect of these basic sites on reaction, pure KF, γ-Al2O3, K3AlF6, KAlO2 and KOH were tested as catalyst, respectively. As displayed in Table 3, the pure γ-Al2O3 and K3AlF6 had no catalytic activity. In contrast, KF, KAlO2 and KOH could promote the conversion of glycerol efficiently. According to our previous work and the opened literature,28,37 it can be confirmed that [Al-OH···F-], KAlO2 and KOH should be the main active species on KF/γ-Al2O3 catalyst for GC synthesis.
Catalyst stability
The stability of a solid base catalyst is a very important factor for its industrial application. The potassium cation leaching from KF/γ-Al2O3 catalysts has been reported in the literature.38 The cation leaching in the form of homogeneous phase can lead to catalyst deactivation, product contamination and limit the catalyst reutilization in a subsequent batch process.39 Thus, it is important to investigate if the K leached from KF/γ-Al2O3 could form active homogeneous species in the solution. For that, the KF/γ-Al2O3 catalyst was filtrated off after 1.0 h of reaction time (73% of glycerol conversion) and then the reaction was continued for 0.5 h. A conversion of 80.2% was obtained. It seemed that part of active species might leach from the catalyst and perform as homogeneous ones. However, the glycerol conversion was lower than that of reaction without removal of catalyst at the same reaction time, demonstrating that the filtrated catalyst performed catalytic activity in the form of heterogeneous phase and played more important role in glycerol conversion as compared with the leached active species. Thus, the heterogeneous phase was the main active species for glycerol conversion.
The recycling of 15% KF/γ-Al2O3 was executed because of its high catalytic activity and GC selectivity. The operation procedure was described in sections Catalytic reaction and Procedure for recycling the catalyst. The results are displayed in Table 4. It was shown that the glycerol conversion and GC selectivity were basically unchanged when the catalyst was reused once. The glycerol conversion decreased in the continued recycling. Generally, the deactivation of catalyst results from the coverage of active site, sintering of the active phase, poisoning of active center and the loss of active ingredient.40 To find the truth of catalyst deactivation, N2 adsorption, XPS characterizations were performed.
The surface area and pore volume of the fresh and reused catalysts are given in Table 5. The first recycling gave similar activity to that of the fresh catalyst, although it possessed a lower surface area and pore volume. The reduction of the surface area and pore volume was mainly ascribed to the blockage of the catalyst microspore by the residual products, which could not be removed entirely by washing with methanol. The sintering of active phase on the catalyst surface could be ignored because of the low reaction temperature. The XPS analysis data of the fresh and recycled catalysts are given in Table 6. It could be seen that K abundance on the catalyst surface decreased gradually with the recycling times. Moreover, the formed methanol stayed in the reaction solution would dissolve KOH and partial KAlO2 on the catalyst surface gradually. The violent stirring during reaction would further enhance the dissolution rate and lead to the accelerated deactivation of the reused catalyst. Thus, the potassium leaching should be the main reason for the catalyst deactivation.
As mentioned above, the thermal treatment temperature for KF/γ-Al2O3 affected GC formation slightly at the temperature 100-400ºC, because the formed new basic sites, KOH and KAlO2 compensated the loss of coordinately unsaturated F- ion at higher temperatures. However, KF/γ-Al2O3 dried at 100 ºC exhibited lower stability than that calcined at 400 ºC. For the first recycling of 15 wt.% KF/γ-Al2O3 treated at 100ºC, the glycerol conversion decreased from 96.2% to 60.8% over fresh catalyst, indicating that the active coordinately unsaturated F- ion was not stable. In contrast, KF/γ-Al2O3 calcined at 400 ºC showed much higher stability. Glycerol conversion of 90.6% and 85.9% of GC yield were obtained at the fourth recycling. This should be attributed to the formation of new stable KAlO2 phases.
Proposed mechanism for transesterification of glycerol and DMC
Ochoa-Gómez et al.16 had suggested that basic catalyst with enough basic strength could activate the primary hydroxyl group of glycerol and proposed a reasonable reaction mechanism accordingly. As the reaction by-products, glycidol and glycerol dicarbonate were detected in the mixed products. Gade41 and Rokicki7 disclosed the formation of glycidol and glycerol dicarbonate in their research work, respectively. However, few research efforts concerned about the effect of formed methanol and glycidol. We found that glycerol and DMC could be formed in the reaction of GC and methanol, indicating that the reaction of glycerol with DMC was reversible. Thus, it was advised to remove the formed methanol in order to improve the glycerol conversion.
As to the formation of glycidol, there existed two possible routes. The one resulted from the decomposition of GC, the other was from the direct dehydration of glycerol. For that, the mixture of glycerol and catalyst was heated to 80 ºC and kept for 1.5 h. GC, glycidol, glycerol dicarbonate were not detected in the product, indicating that the formation of glycidol was from the decomposition of GC rather than the direct dehydration of glycerol. Furthermore, the interaction42 of epoxy group with carbon dioxide could confirm that formation of glycidol from GC was also a reversible reaction.
Based on the properties of basic catalyst and product distribution, we proposed a possible mechanism (shown in Figure 5) for the transesterification of glycerol and DMC. The first four steps of possible reaction mechanism illustrated in Figure 5 were similar to the one in reference.16 However, GC could react reversibly with methanol and produce glycerol. Furthermore, as the side reactions, GC could not only be decomposed to glycidol and CO2, but also react with the excessive DMC to glycerol dicarbonate.
Conclusions
In summary, KF/γ-Al2O3 prepared by a wet impregnation way is an efficient solid base catalyst for the synthesis of GC from glycerol and DMC. It was proved that [Al-OH···F-], KOH and KAlO2 were the main active basic sites for GC formation. Furthermore, it was obtained that the strong basic sites not only promoted the conversion of glycerol, but also enhanced the decomposition of GC into glycidol. The deactivation of the catalyst was mainly caused by the leaching of active potassium species. Moreover, elevating the calcination temperature of KF/γ-Al2O3 could retard the deactivation rate. Based on the product distribution, a possible catalytic reaction mechanism was proposed.
Acknowledgments
We thank the National Key Basic Research and Development Program of China for financial support (Project No. 2012CB215305).
Submitted: August 2, 2013
Published online: November 29, 2013
- 1. Zhou, C. H.; Beltramini, J. N.; Fan, Y. X.; Lu, G. Q.; Chem. Soc. Rev. 2008,37,527.
- 2. da Silva, G. P.; Mack, M.; Contiero, J.; Biotechnol. Adv. 2009,27,30.
- 3. Dasari, M. A.; Kiatsimkul, P. -P.; Sutterlin, W. R.; Suppes, G. J.; Appl. Catal. A: Gen. 2005,281,225.
- 4. Pagliaro, M.; Ciriminna, R.; Kimura, H.; Rossi, M.; Della Pina, C.; Angew. Chem., Int. Ed. 2007,46,4434.
- 5. Sonnati, M. O.; Amigoni, S.; de Givenchy, E. P. T.; Darmanin, T.; Choulet, O.; Guittard, F.; Green Chem. 2013,15,283.
- 6. Ubaghs, L.; Fricke, N.; Keul, H.; Höcker, H.; Macromol. Rapid Commun. 2004,25,517.
- 7. Rokicki, G.; Rakoczy, P.; Parzuchowski, P.; Sobiecki, M.; Green Chem. 2005,7,529.
- 8. Mei, H.; Zhong, Z.; Long, F.; Zhuo, R.; Macromol. Rapid Commun. 2006,27,1894.
- 9. Burk, R. M.; Roof, M. B.; Tetrahedron Lett. 1993,34,395.
- 10. Mizuno, T.; Nakai, T.; Mihara, M.; Heteroat. Chem. 2010, 21,99.
- 11. Hu, J.; Li, J.; Gu, Y.; Guan, Z.; Mo, W.; Ni, Y.; Li, T.; Li, G.; Appl. Catal. A: Gen. 2010,386,188.
- 12. Vieville, C.; Yoo, J.; Pelet, S.; Mouloungui, Z.; Catal. Lett. 1998,56,245.
- 13. George, J.; Patel, Y.; Pillai, S. M.; Munshi, P.; J. Mol. Catal. A: Chem. 2009,304,1.
- 14. Climent, M. J.; Corma, A.; De Frutos, P.; Iborra, S.; Noy, M.; Velty, A.; Concepción, P.; J. Catal. 2010,269,140.
- 15. Hammond, C.; Lopez-Sanchez, J. A.; Ab Rahim, M. H.; Dimitratos, N.; Jenkins, R. L.; Carley, A. F.; He, Q.; Kiely, C. J.; Knight, D. W.; Hutchings, G. J.; Dalton Trans. 2011,40,3927.
- 16. Ochoa-Gómez, J. R.; Gómez-Jiménez-Aberasturi, O.; Maestro-Madurga, B.; Pesquera-Rodríguez, A.; Ramírez-López, C.; Lorenzo-Ibarreta, L.; Torrecilla-Soria, J.; Villarán-Velasco, M. C.; Appl. Catal. A: Gen. 2009,366,315.
- 17. Bell, J. B.; US Pat. 2,915,529 1959
- 18. Alvarez, M. G.; Segarra, A. M.; Contreras, S.; Sueiras, J. E.; Medina, F.; Figueras, F.; Chem. Eng. J. 2010,161,340.
- 19. Bai, R.; Wang, Y.; Wang, S.; Mei, F.; Li, T.; Li, G.; Fuel Process. Technol. 2013,106,209.
- 20. Kim, S. C.; Kim, Y. H.; Lee, H.; Yoon, D. Y.; Song, B. K.; J. Mol. Catal. B: Enzym. 2007,49,75.
- 21. Grey, R. A.; US Pat. 5,091,543 1992
- 22. Naik, P. U.; Petitjean, L.; Refes, K.; Picquet, M.; Plasseraud, L.; Adv. Synth. Catal. 2009,351,1753.
- 23. Takagaki, A.; Iwatani, K.; Nishimura, S.; Ebitani, K.; Green Chem. 2010,12,578.
- 24. Clark, J. H.; Chem. Rev. 1980,80,429.
- 25. Ando, T.; Brown, S. J.; Clark, J. H.; Cork, D. G.; Hanafusa, T.; Ichihara, J.; Miller, J. M.; Robertson, M. S.; J. Chem. Soc., Perkin Trans. 2 1986,1133.
- 26. Wen, L.; Ji, C.; Li, Y.; Li, M.; J. Comb. Chem. 2009,11,799.
- 27. Qiu, P.; Yang, B.; Yi, C.; Qi, S.; Catal. Lett. 2010,137,232.
- 28. Ando, T.; Clark, J. H.; Cork, D. G.; Hanafusa, T.; Ichihara, J.; Kimura, T.; Tetrahedron Lett. 1987,28,1421.
- 29. Vazquez, A.; Lopez, T.; Gomez, R.; Morales, A.; Novaro, O.; J. Solid State Chem. 1997,128,161.
- 30. Xie, W.; Peng, H.; Chen, L.; Appl. Catal. A: Gen. 2006,300,67.
- 31. Hoydonckx, H. E.; De Vos, D. E.; Chavan, S. A.; Jacobs, P. A.; Top. Catal. 2004,27,83.
- 32. Gerpen, J. V.; Fuel Process. Technol. 2005,86,1097.
- 33. Tanabe, K. In Catalysis by Acids and Bases; Tanabe, K.; Imelik, B., eds.; Elsevier: Amsterdam, 1985.
- 34. Wan, T.; Yu, P.; Gong, S.; Li, Q.; Luo, Y.; Korean J. Chem. Eng. 2008,25,998.
- 35. Murugan, C.; Bajaj, H.; Fuel Process. Technol. 2011,92,77.
- 36. Zhu, J. H.; Xu, Q. H.; Acta Chim. Sinica 1997,55,474.
- 37. Verziu, M.; Florea, M.; Simon, S.; Simon, V.; Filip, P.; Parvulescu, V. I.; Hardacre, C.; J. Catal. 2009,263,56.
- 38. Alonso, D. M.; Mariscal, R.; Moreno-Tost, R.; Poves, M.; Granados, M. L.; Catal. Commun. 2007,8,2074.
- 39. Castro, C. S.; Cardoso, D.; Nascente, P. A.; Assaf, J. M.; Catal. Lett. 2011,141,1316.
- 40. Di Serio, M.; Mallardo, S.; Carotenuto, G.; Tesser, R.; Santacesaria, E.; Catal. Today 2012,195,54.
- 41. Gade, S. M.; Munshi, M. K.; Chherawalla, B. M.; Rane, V. H.; Kelkar, A. A.; Catal. Commun. 2012,27,184.
- 42. Li, Z.; Zhao, Y.; Yan, S.; Wang, X.; Kang, M.; Wang, J.; Xiang, H.; Catal. Lett. 2008,123,246.
Publication Dates
-
Publication in this collection
28 Jan 2014 -
Date of issue
Jan 2014
History
-
Received
02 Aug 2013 -
Accepted
29 Nov 2013