Acessibilidade / Reportar erro

Quantification by FT-IR (UATR/NIRA) of NBR/SBR blends

Abstract

Rubber blends are important materials in automotive industry, as well as in other sectors. However, there are implications when suitable use of a polymer in an artifact is not made. In the automotive area, for example, the use of an elastomer without the fuel resistance requirement would result in component degradation, potential fuel leakage, and danger of fire. The use of polymer blends may be the solution to this problem. Fourier transform infrared spectroscopy (FT-IR) can be used for the knowledge of the polymer content of these blends. Then, FT-IR quantitative methodologies for determining acrylonitrile-butadiene copolymer (NBR) copolymer and butadiene-styrene copolymer (SBR) contents were developed by the transflectance accessory, NIRA, and the transmission mode, being the sample analyzed by transmission and universal attenuated total reflection (UATR) in the medium infrared (MIR). UATR and NIRA methodologies showed better accuracy. However, the MIR analysis showed a detection limit between 10-20% of NBR.

Keywords:
content; NBR; NIRA; SBR; UATR

1. Introduction

In contrast to the deceleration in the new polymers production, there is a growing interest in the processes research and development for the modification of existing polymers[11 Hemais, C. A., Rosa, E. O. R., & Barros, H. M. (2000). Observações sobre desenvolvimentos Tecnológicos e os ciclos da Industria de Polímeros do Brasil. Polímeros: Ciência e Tecnologia, 10(3), 149-154. http://dx.doi.org/10.1590/S0104-14282000000300011.
http://dx.doi.org/10.1590/S0104-1428200...
]. In this context, polymer blends are available for specific applications. According to the literature, the necessary condition is that the lower content of one of components must exceed at least 5%[22 Simielli, E. R. (1993). Principais características das blendas poliméricas fabricadas no Brasil. Polímeros: Ciência e Tecnologia , 3(1), 45-49. Retrieved in 2018, January 12, from http://www.revistapolimeros.org.br/pdf/v3n1/v3n1a06.pdf
http://www.revistapolimeros.org.br/pdf/...
,33 Ramesan, M. T., Kuriakose, B., Pradeep, P., Alex, R., & Varghese, S. (2001). Compatibilization of SBR/NBR blends using chemically modified styrene butadiene rubber. International Polymer Processing, 16(2), 183-191. http://dx.doi.org/10.3139/217.1640.
http://dx.doi.org/10.3139/217.1640 ...
].

Blends are often used to improve properties of each polymer involved in the product, process and/or reduce cost. There are many applications in several industries, such as aeronautics, naval, automotive, graphics, real estate, among others. Therefore, studies involving polymers and their blends are attractive, since the methodologies developed can be used in different sectors[11 Hemais, C. A., Rosa, E. O. R., & Barros, H. M. (2000). Observações sobre desenvolvimentos Tecnológicos e os ciclos da Industria de Polímeros do Brasil. Polímeros: Ciência e Tecnologia, 10(3), 149-154. http://dx.doi.org/10.1590/S0104-14282000000300011.
http://dx.doi.org/10.1590/S0104-1428200...
,44 Alcantara, A. F., Nunes, R. C. R., & Visconte, L. L. Y. (2004). Mistura BR/SBR: propriedades mecânicas em função de modo de preparo. Polímeros: Ciência e Tecnologia, 14(4), 279-282. http://dx.doi.org/10.1590/S0104-14282004000400015.
http://dx.doi.org/10.1590/S0104-1428200...
].

Butadiene-based copolymers are widely used in automotive industry. Among these, the SBR and NBR copolymers are outstanding. SBR plays a major role in the market due to its application in tires production. When SBR is used in conjunction with the BR-high cis butadiene homopolymer, excellent properties are obtained for application to tire tread. Since year 2000, automobile and tire manufacturers have been concerned about the environment and which led them to invest in new cleaner synthetic processes for production of these elastomers. Butadiene is a monomer used in the manufacture of elastomers of great economic interest worldwide. According to their properties, the polymers are assigned to a specific type of use[55 Rocha, T. C. J., Soares, B. G., & Coutinho, F. M. B. (2007). Principais copolímeros elastoméricos à base de butadieno utilizados na indústria automobilística. Polímeros: Ciência e Tecnologia, 17(4), 299-307. http://dx.doi.org/10.1590/S0104-14282007000400009.
http://dx.doi.org/10.1590/S0104-1428200...
].

There are several blends available in the world market, but for the purpose of this paper, the blend composed of NBR and SBR copolymers was selected based on its properties which are suitable on lowering costs by improving certain properties of NBR rubber, which has good chemical and oil resistance. However, these properties vary according to a considerable number of rubber products. Higher the acrylonitrile (AN) content, greater the oil resistance, however lower the flexibility. It is possible to use a NBR blend of high content AN with SBR rubber to obtain an oil resistance degree as such a NBR with low content of AN, with an overall economy in cost. NBR products with high AN content tends to shrink in contact with lubricating oils, in high temperature. The manufacture of NBR/SBR blends constitutes a solution for the final artifact achieve desired properties. SBR can also improve NBR processing[66 Ramesan, M. T., & Alex, R. (2001). Compatibilization of SBR/NBR blends using chemically modified styrene-co-butadiene rubber - Part 2. Effect of compatibilizer loading. Polymer International, 50(12), 1298-1308. http://dx.doi.org/10.1002/pi.775.
http://dx.doi.org/10.1002/pi.775 ...
].

In the automotive industry, NBR is usually applied in hoses that have direct contact with fuels or gases [55 Rocha, T. C. J., Soares, B. G., & Coutinho, F. M. B. (2007). Principais copolímeros elastoméricos à base de butadieno utilizados na indústria automobilística. Polímeros: Ciência e Tecnologia, 17(4), 299-307. http://dx.doi.org/10.1590/S0104-14282007000400009.
http://dx.doi.org/10.1590/S0104-1428200...
]. NBR is also used in the aerospace industry, as rocket motor thermal insulation [77 Pedreira, S. M., Pinto, J. R. A., Campos, E. A., Mattos, E. D. C., Oliveira, M. S., Jr., Oliveira, J. I. S., & Dutra, R. D. C. L. (2016). Methodologies for characterization of aerospace polymers/energetic materials – a short review. Journal of Aerospace Technology and Management, 8(1), 18-25. http://dx.doi.org/10.5028/jatm.v8i1.576.
http://dx.doi.org/10.5028/jatm.v8i1.576...
]. It comes to our attention that the quality of the product delivered by the supplier might not meet the specification needed, consisting only by NBR. This may lead to detachments compromising the integrity of the rubber / propellant interface.

NBR rubber also benefits aeronautics industry on appliances as such hoses, seals, and self-sealing fuel and oil tanks. It is applied in the nuclear industry to make protective gloves. NBR property of withstanding a temperature range of -40 to 108°C makes it the ideal material for aeronautical applications. Still, NBR can be applied to create molded products, adhesives, sealants, sponges, expanded foams and carpets[88 Wikipedia. (2018). Nitrile rubber. Retrieved in 2018, January 12, from https://en.wikipedia.org/wiki/Nitrile_rubber
https://en.wikipedia.org/wiki/Nitrile_r...
].

A variation in polymerization, AN ratio to butadiene, processing properties and vulcanization are characteristics added in NBR / SBR blend by NBR rubber worth to mention. The AN content is one of the main criteria to define the basic properties of an elastomer. Nitrile group polarity grants to elastomers resistance to oils and hydrocarbon-based solvents, flexibility and abrasion resistance[55 Rocha, T. C. J., Soares, B. G., & Coutinho, F. M. B. (2007). Principais copolímeros elastoméricos à base de butadieno utilizados na indústria automobilística. Polímeros: Ciência e Tecnologia, 17(4), 299-307. http://dx.doi.org/10.1590/S0104-14282007000400009.
http://dx.doi.org/10.1590/S0104-1428200...
]. In this paper, a NBR rubber with AN content of 37-41% was used according to NBR supplier. Additionally, a FT-IR methodology developed by the group[99 Sanches, N. B., Diniz, M. F., Alves, L. C., Dutra, J. C. N., Cassu, S. N., Azevedo, M. F. P., Mattos, E. C., & Dutra, R. C. L. (2008). Avaliação da aplicabilidade de técnicas FT-IR de reflexão (UATR) e de transmissão para a determinação do teor de acrilonitrila (AN) em NBR. Polímeros: Ciência e Tecnologia , 18(3), 249-255. http://dx.doi.org/10.1590/S0104-14282008000300011.
http://dx.doi.org/10.1590/S0104-1428200...
] was applied to precisely acquire the AN value.

The AN content determination in NBR have been performed by FT-IR transmission with values reference obtained by Kjeldhal method[1010 Chakraborty, S., Bandyopadhyay, S., Ameta, R., Mukhopadhyay, R., & Deuri, A. S. (2007). Application of FTIR in characterization of acrylonitrile-butadiene rubber (nitrile rubber). Polymer Testing, 26(1), 38-41. http://dx.doi.org/10.1016/j.polymertesting.2006.08.004.
http://dx.doi.org/10.1016/j.polymertest...
], measuring contents up to around 40%. FT-IR transmission and reflection (UATR) techniques[99 Sanches, N. B., Diniz, M. F., Alves, L. C., Dutra, J. C. N., Cassu, S. N., Azevedo, M. F. P., Mattos, E. C., & Dutra, R. C. L. (2008). Avaliação da aplicabilidade de técnicas FT-IR de reflexão (UATR) e de transmissão para a determinação do teor de acrilonitrila (AN) em NBR. Polímeros: Ciência e Tecnologia , 18(3), 249-255. http://dx.doi.org/10.1590/S0104-14282008000300011.
http://dx.doi.org/10.1590/S0104-1428200...
] were used for determining contents up to around 50%, with good results, indicating that UATR methodology presents better linear correlation and less analysis time.

One of the most common blend elastomer is the SBR responsible for nearly 40% of all synthetic rubber used in the world. According to data from 2007, approximately 2.4 million tons of SBR per year were already produced in the world[55 Rocha, T. C. J., Soares, B. G., & Coutinho, F. M. B. (2007). Principais copolímeros elastoméricos à base de butadieno utilizados na indústria automobilística. Polímeros: Ciência e Tecnologia, 17(4), 299-307. http://dx.doi.org/10.1590/S0104-14282007000400009.
http://dx.doi.org/10.1590/S0104-1428200...
]. SBR rubber characteristics depend on styrene content, which can vary between 10 and 85%. Formulations with low styrene content exhibit an elastomeric behavior, whereas those with high styrene content have a thermoplastic nature[1111 Ghebremeskel, G. N., Sekinger, J. K., Hoffpauir, J. L., & Hendrix, C. (1996). A study on the thermal degradation products of styrene-butadiene type rubber by pyrolysis/GC/MS. Rubber Chemistry and Technology, 69(5), 874-884. http://dx.doi.org/10.5254/1.3538409.
http://dx.doi.org/10.5254/1.3538409 ...
]. SBR-1502 was object of this study, with 23.5% styrene, obtained by cold polymerization (10°C maximum) in emulsion of fatty and resinous soaps, coagulated in a salt / acid or acid system and stabilized with a non-smelly antioxidant.

SBR rubber has good mechanical properties, high resistance. Likewise, it has good resistance to abrasion, ozone and weathering, but regarding to oil resistance it presents a gap, making this mixture with NBR beneficial for both copolymers, dependent on the suitable application of the final artifact[1212 Yehia, A. A., Mansour, A. A., & Stoll, B. (1997). Detection of compatibility of some rubber blends by DSC. Journal of Thermal Analysis, 48(6), 1299-1310. http://dx.doi.org/10.1007/BF01983440.
http://dx.doi.org/10.1007/BF01983440 ...
].

The property variations are dependent on the functional groups content of the polymers and also compounds present in the product composition. Therefore, the possibility of using blends to reach a specific application indicates the need for suitable characterization and/or quantification of these materials. Instrumental techniques, mainly Fourier transform infrared spectroscopy (FT-IR), associated or not with other techniques, is mentioned in the literature for this goal, including also studies of polymers used in the automotive and aerospace industry, such as NBR, SBR and their polymer blends[1313 Ferreira, A. C., Diniz, M. F., & Mattos, E. C. (2018). FT-IR methodology transmission and UATR for quantifying automotive systems. Polímeros: Ciência e Tecnologia, 28(1), 6-14. http://dx.doi.org/10.1590/0104-1428.2412.
http://dx.doi.org/10.1590/0104-1428.241...

14 Choi, S.-S., Kim, Y., & Kwon, H.-M. (2014). Microstructural analysis and cis–transisomerization of BR and SBR vulcanizates reinforced with silica and carbon black using NMR and IR. RSC Advances, 4(59), 31113-31119. http://dx.doi.org/10.1039/C4RA03682D.
http://dx.doi.org/10.1039/C4RA03682D ...

15 Perez, L. D., & Lopez, B. L. (2012). Thermal characterization of SBR/NBR blends reinforced with a mesoporous silica. Journal of Applied Polymer Science, 125(S1), E327-E333. http://dx.doi.org/10.1002/app.35689.
http://dx.doi.org/10.1002/app.35689 ...

16 Noriman, N. Z., Ismail, H., & Rashid, A. A. (2010). Characterization of styrene butadiene rubber/recycled acrylonitrile-butadiene rubber (SBR/NBRr) blends: The effects of epoxidized natural rubber (ENR-50) as a compatibilizer. Polymer Testing, 29(2), 200-208. http://dx.doi.org/10.1016/j.polymertesting.2009.11.002.
http://dx.doi.org/10.1016/j.polymertest...

17 Dutra, R. C. L., Diniz, M. F., Ribeiro, A. P., Lourenço, V. L., Cassu, S. N., & Azevedo, M. P. (2004). Determinação do teor de NR/SBR em misturas: associação de dados DTG e FT-IR e/ou ensaios auxiliares. Polímeros: Ciência e Tecnologia, 14(5), 334-338. http://dx.doi.org/10.1590/S0104-14282004000500011.
http://dx.doi.org/10.1590/S0104-1428200...
-1818 Shield, S. R., Ghebremeskel, G. N., & Hendrix, C. (2001). Pyrolysis-GC/MS and TGA as tools for characterizing blends of SBR and NBR. Rubber Chemistry and Technology , 74(5), 803-813. http://dx.doi.org/10.5254/1.3547654.
http://dx.doi.org/10.5254/1.3547654 ...
].

Table 1 shows some studies. Although good results were achieved in these studies, some observations were made in this study, which served as a basis for the elaboration of the methodology currently developed.

Table 1
Main aspects cited by studies on polymers and their blends characterization.

It is observed that the MIR region is the most used, just as the technique obtaining FT-IR spectra is the conventional one, which means transmission and the use of other instrumental techniques. However, it validates the FT-IR data and makes the methodology more complex and time-consuming. Methodological errors are not generally compared. In this paper, it was proposed a FT-IR methodology in the MIR region, with data validation in the NIR region, by means of less conventional spectral modes, such as UATR and NIRA, compared to data obtained by transmission. The samples were prepared by pyrolysis in a Bunsen burner, with evaluation of FT-IR methodology error.

2. Materials and Methods

2.1 Samples

Nine samples of NBR/SBR blends were prepared at Tenneco Automotive Brazil, with materials kindly provided by the company, in the proportions 10/90, 20/80, 30/70, 40/60, 50/50, 60/40, 70/30, 80/20, 90/10, according to the formulation found in Table 2 .

Table 2
NBR/SBR Blend Formulation System.

2.1.1 Preparation of rubber samples

The raw material was weighed on a precision scale and all components, except sulfur and accelerators, tetramethylthiuram disulfide (TMTD), (1,3-Dimethylbutyl)-N'-phenyl-phenylenediamine (6PPD), N-(cyclohexylthio) phthalimide (PVI) and 4,4 Dithiomorpholine (DTDM), which were mixed in banbury of 2 liters per 240 seconds, with a pound pressure of 4 kgf/cm2 , rotation of 70 rpm and initial temperature of 40°C, for production of master batch. It was processed into a roller form six times in a lab open mill with a rotation of 40 rpm. Later, the master batch was accelerated at banbury, with the rest of the weighted components (TMTD, 6PPD, PVI, DTDM and sulfur) for 120 seconds, with 4kgf/cm2 pound pressure, 70 rpm rotation and initial temperature of 40° C. Then the rubber was homogenized in roller form six times in an open mil lab with a rotation of 40 rpm and withdrawn into blanked. For the preparation of vulcanized rubber sheet, a hydraulic press with vulcanization time of 6 min, plateaus temperature of 160°C and 150 kgf/cm2 of closing pressure was used.

2.2 Equipment of characterization/conditions

2.2.1 FT-IR analysis

The samples were analyzed in Spectrum One PERKINELMER FT-IR spectrometer (MIR regions of 4000 to 400 cm-1 and NIR of 12000 to 4000 cm-1, 4 cm-1 resolutions, gain 1, 20 scans), being spectra obtained by transmission techniques (MIR and NIR) and reflection (MIR), using the UATR accessory, and in NIR region, also using the Frontier PERKINELMER FT-IR spectrometer, NIRA accessory, being all samples of different methodologies, prepared by pyrolysis in Bunsen burner.

In Bunsen's pyrolysis, samples of each rubber blend were cut, extracted for 8 hours in a Soxhlet extractor, using methanol as solvent[2525 Wake, W. C., Tidd, B. K., & Loadman, M. J. R. (1983). Analysis of rubber and rubber-like polymer. 3rd ed. New York: Applied Science. ]. After solvent evaporation in the oven, it was put a quantity of about 0.5 g of sample in each pyrolysis tube. The tubes were flamed in Bunsen burner, at the same flame height (marked with the aid of an universal device and a claw to determine the same pyrolysis position). For the transmission analysis, by pyrolysis, was used the 0.025mm spacer.

By reflection, using the UATR accessory, in the same way that was done in a recent study by Rigoli et al.[2626 Rigoli, P. S., Murakami, L. M. S., Diniz, M. F., Azevedo, M. F. P., Cassu, S. N., Mattos, E. C., & Dutra, R. C. L. (In press). Quantification of aerospace polymer blends by thermogravimetric analysis and infrared spectrometry. Journal of Aerospace Technology and Management . ], the pyrolysis samples were analyzed by placing them in contact with the diamond-coated zinc selenide crystal surface with 120N (Newton) torque application.

For MIR analysis, the nine NBR/SBR samples (composition already shown in Table 2 ), prepared by pyrolysis in Bunsen burner and analyzed by transmission and reflection (UATR), were used to prepare ANBR/ASBR x [NBR]/[SBR] analytical curve, aiming the NBR and SBR contents determination, through the relative band A2237 /A700. This band is composed by analytical absorptions of stretching (υ) C ≡N of NBR (2237 cm-1) and bending (δ) C-H of SBR (700 cm -1). The baselines used were: 2275-2150 cm-1 (band 2237 cm-1 ) and 2150-590 cm-1 (band 700 cm-1), for transmission / pyrolysis methodology, and 2275-2180 cm-1 (band 2237 cm -1), 858-642 cm -1 (band 700 cm-1) for UATR methodology.

For the NIR methodology, the same number of reference NBR / SBR samples, prepared by pyrolysis in Bunsen burner and analyzed by transmission, were used to prepare the analytical curve A4336/A4060 x [NBR]/[SBR]. The bands chosen are in the region of combination or overtones of fundamental bands. In the case of NBR/SBR blend, the band A4336 is probably attributed to the first overtone of stretching (υ) of C≡N group of NBR or of combination bands, and the A4060 to the second overtone of bending (δ) of SBR aromatic CH groups[1919 Shield, S. R., & Ghebremeskel, G. M. (2003). Use of mid and near infrared techniques as tools for characterizing blends of copolymers of styrene–butadiene and acrylonitrile-butadiene. Journal of Applied Polymer Science, 88(7), 1653-1658. http://dx.doi.org/10.1002/app.11849.
http://dx.doi.org/10.1002/app.11849 ...
,2727 Goddu, R. F. (1960). Near-infrared spectrophotometry. In C. N. Reilly (Ed.), Advances in analytical chemistry and instrumentation (pp. 347-425). New York: Interscience. ]. The baseline used was 4540-4000 cm-1 (bands 4336 and 4060 cm -1). For NIRA methodology, the same number of samples and the same analytical bands were used. The samples were also prepared by pyrolysis in Bunsen burner, and were analyzed by transflectance because they were in the liquid state[2828 Mello, T. S. D., Diniz, M. F., & Dutra, R. C. L. (2018). UATR and NIRA evaluation in the quantification of ATBC in NC blends. Polímeros: Ciência e Tecnologia , 28(3), 239-245. http://dx.doi.org/10.1590/0104-1428.16816.
http://dx.doi.org/10.1590/0104-1428.168...
]. The baseline used was 4780 to 4000 cm-1.

The data of all FT-IR/MIR and NIR methodologies, for each sample, represent the median of 5 values of analytical bands intensity chosen, being that the mean standard deviations ( Equations 1 and 2 ) and the relative error (RD) ( Equation 3 ) were calculated by non-parametric treatment in agreement with Hórak[2929 Horák, V. M., & Vítek, A. (1978). Interpretation and processing of vibrational spectra. New York: John Wiley & Sons. ] and with the methodology adopted successfully in group quantitative studies for rubber and other materials[1717 Dutra, R. C. L., Diniz, M. F., Ribeiro, A. P., Lourenço, V. L., Cassu, S. N., & Azevedo, M. P. (2004). Determinação do teor de NR/SBR em misturas: associação de dados DTG e FT-IR e/ou ensaios auxiliares. Polímeros: Ciência e Tecnologia, 14(5), 334-338. http://dx.doi.org/10.1590/S0104-14282004000500011.
http://dx.doi.org/10.1590/S0104-1428200...
,2828 Mello, T. S. D., Diniz, M. F., & Dutra, R. C. L. (2018). UATR and NIRA evaluation in the quantification of ATBC in NC blends. Polímeros: Ciência e Tecnologia , 28(3), 239-245. http://dx.doi.org/10.1590/0104-1428.16816.
http://dx.doi.org/10.1590/0104-1428.168...
,3030 Damazio, D., Santos, R. P., Diniz, M. F., & Dutra, R. C. L. (2015). Determinação do teor de ENB em EPDM (elastômero puro) por FT-IR de transmissão, por meio de banda relativa. Polímeros: Ciência e Tecnologia, 25(2), 181-185. http://dx.doi.org/10.1590/0104-1428.1777.
http://dx.doi.org/10.1590/0104-1428.177...
].

σ ^ μ ^ = σ ^ n (1)
σ ^ = K R × R (2)

Where, σ^ is the mean standard deviation, n, the measurements number, R is the difference between the highest and the lowest values of absorbance. KR is the coefficient to calculate the standard deviation ( σ^ ) of a range of values, with KR = 0.430 for 5 experiments[2929 Horák, V. M., & Vítek, A. (1978). Interpretation and processing of vibrational spectra. New York: John Wiley & Sons. ]. The RD of the measurements for each analyzed sample, given in %, was determined by Equation 3 , where μ is the median value of A. The median of the relative errors represents the error of the methodology[1717 Dutra, R. C. L., Diniz, M. F., Ribeiro, A. P., Lourenço, V. L., Cassu, S. N., & Azevedo, M. P. (2004). Determinação do teor de NR/SBR em misturas: associação de dados DTG e FT-IR e/ou ensaios auxiliares. Polímeros: Ciência e Tecnologia, 14(5), 334-338. http://dx.doi.org/10.1590/S0104-14282004000500011.
http://dx.doi.org/10.1590/S0104-1428200...
,2828 Mello, T. S. D., Diniz, M. F., & Dutra, R. C. L. (2018). UATR and NIRA evaluation in the quantification of ATBC in NC blends. Polímeros: Ciência e Tecnologia , 28(3), 239-245. http://dx.doi.org/10.1590/0104-1428.16816.
http://dx.doi.org/10.1590/0104-1428.168...
,3030 Damazio, D., Santos, R. P., Diniz, M. F., & Dutra, R. C. L. (2015). Determinação do teor de ENB em EPDM (elastômero puro) por FT-IR de transmissão, por meio de banda relativa. Polímeros: Ciência e Tecnologia, 25(2), 181-185. http://dx.doi.org/10.1590/0104-1428.1777.
http://dx.doi.org/10.1590/0104-1428.177...
].

R D ( % ) = σ ^ μ ^ μ × 100 (3)

3. Results and Discussion

3.1 FT-IR analysis

In this topic the following were addressed: a) the determination by UATR of AN content of NBR used in the blends, according to methodology previously developed by the group[99 Sanches, N. B., Diniz, M. F., Alves, L. C., Dutra, J. C. N., Cassu, S. N., Azevedo, M. F. P., Mattos, E. C., & Dutra, R. C. L. (2008). Avaliação da aplicabilidade de técnicas FT-IR de reflexão (UATR) e de transmissão para a determinação do teor de acrilonitrila (AN) em NBR. Polímeros: Ciência e Tecnologia , 18(3), 249-255. http://dx.doi.org/10.1590/S0104-14282008000300011.
http://dx.doi.org/10.1590/S0104-1428200...
], since only one range was furnished by the supplier. For SBR rubber, the determined value as reported by the supplier was used. These values were not used in the blends contents calculation, only used for the proper characterization of the raw materials used for the prediction of properties of blends, for future and specific applications. b) the determination of the NBR/SBR blends in two spectral regions, by different ways of obtaining spectra, aiming to evaluate the most suitable conditions for this type of analysis.

3.2 Determination by UATR of AN content of NBR used in the blend

In Table 3 , the data for AN content in NBR calculation are inserted.

Table 3
UATR data for determination of AN in NBR.

3.3 MIR/transmission analysis of NBR/SBR

In Figure 1 , are the MIR/transmission spectra of some NBR/SBR blends studied. It can be observed that the bands intensities A2237 and A700 increase and decrease according to the content of NBR and SBR, respectively, as expected by Lambert-Beer Law, for quantitative analyzes[3232 Smith, A. L. (1979). Applied infrared spectroscopy. New York: John Wiley & Sons. ]. The data for elaboration of calibration curve are shown in Table 4 and Figure 2 . To overcome liquid film thickness issues and to improve the data accuracy[3232 Smith, A. L. (1979). Applied infrared spectroscopy. New York: John Wiley & Sons. ], mean values of relative band A2237/A700 were considered as a function of the relative NBR/SBR concentration.

Figure 1
MIR/transmission spectra (Bunsen burner pyrolysis) of NBR/SBR blends, with AN and styrene bands, marked with n and s, respectively.
Table 4
MIR/transmission data (Bunsen burner pyrolysis) for calibration curve elaboration and associated methodology errors.
Figure 2
MIR/transmission calibration curve A2237/A700 versus relative concentration [NBR/SBR].

From the calibration curve ( Table 4 ), the following correlation ( Equation 4 - R = 0.98, with 96% of the values explained by the methodology, R2 = 0.96) is proposed:

A 2237 / A 700 = 0.17 [ N B R ] / [ S B R ] + 0.14 (4)

To find the two elastomers contents of the unknown mixture, Equation 5 should also be used. This is valid for all the methodologies developed in this study.

[ N B R ] + [ S B R ] = 100 % (5)

The methodology error, which is relative errors median[2828 Mello, T. S. D., Diniz, M. F., & Dutra, R. C. L. (2018). UATR and NIRA evaluation in the quantification of ATBC in NC blends. Polímeros: Ciência e Tecnologia , 28(3), 239-245. http://dx.doi.org/10.1590/0104-1428.16816.
http://dx.doi.org/10.1590/0104-1428.168...
] calculated in Table 4 , already mentioned, 4.18%, can be considered good, compared to the reference value [2929 Horák, V. M., & Vítek, A. (1978). Interpretation and processing of vibrational spectra. New York: John Wiley & Sons. ], ≤ 2%, which is usually only found under fixed conditions, ideal for sample preparation, that is, in solution form and analyzed in closed cell, with thickness control. The error falls to 2.79%, closer to the accuracy limit of the equipment, ≤ 2%, for optimal condition, if the contents of 10-20% of NBR are not considered, may suggest a limit of detection in this range, by this methodology, probably due to the low intensity of the AN band, for these levels.

3.4 MIR/UATR analysis of NBR/SBR

In Figure 3 , the MIR/UATR spectra of some studied NBR/SBR polymer blends are included. As for transmission MIR spectra, it can be observed that the intensities of bands A2237 and A 700 increase and decrease according to the NBR and SBR content, respectively, as expected by the Lambert-Beer Law. The data for calibration curve elaboration are shown in Table 5 and Figure 4 . In this methodology, A2237/A700 relative band was also used to improve the accuracy of the data.

Figure 3
MIR/UATR spectra of NBR/SBR blends, with the AN and styrene bands, labeled with n and s, respectively.
Table 5
MIR/UATR data (Bunsen burner pyrolysis) for calibration curve elaboration and associated methodology errors.
Figure 4
MIR/UATR calibration curve A2237/A700 versus relative concentration [NBR/SBR].

From the calibration curve ( Table 5 ), the following correlation ( Equation 6 - R = 0.98, with 96% of the values explained by the methodology, R2 = 0.96) is proposed:

A 2237 / A 700 = 0.05 [ N B R ] / [ S B R ] + 0.03 (6)

The methodology error, which is the median of the relative errors ( Table 5 ), 3.41%, can be considered good compared to the reference value, ≤ 2%. The error falls to 2.09%, closer to the accuracy limit of the equipment, ≤ 2%, for optimal condition, if the contents of 10-20% of NBR are not considered, and may also suggest a limit of detection in this band, by this methodology, probably due to the low intensity of the AN band, for these levels.

3.5 NIR/transmission analysis of NBR/SBR

In Figure 5 , the NIR/transmission (pyrolysis in Bunsen burner) spectra of some NBR / SBR polymer blends studied are shown. As for MIR and UATR spectra, it can be observed that the intensities of the bands A4336 and A4060 increase and decrease according to the NBR and SBR content, respectively, as expected by the Lambert-Beer Law.

Figure 5
NIR transmission spectra (Bunsen burner pyrolysis) of NBR/SBR blends, with AN and styrene bands, labeled with n and s, respectively.

In this methodology, the relative band A4336/A4060 was chosen to overcome liquid film thickness issues and to improve the data accuracy. Table 6 shows the values used, as well as their mean and relative deviations.

Table 6
NIR transmission data (Bunsen burner pyrolysis) for calibration curve elaboration and associated methodology errors.

Figure 6 shows the calibration curve of NIR / transmission (Bunsen burner pyrolysis) A4336 /A4060 versus [NBR]/[SBR] (% w/w). From the calibration curve ( Table 6 ), the following correlation ( Equation 7 - R = 0.92, with 85% of the values found, being explained by the developed methodology) is proposed:

Figure 6
NIR calibration curve A4436/A4060 versus relative concentration [NBR/SBR].
A 4336 / A 4060 = 0.26 [ N B R ] / [ S B R ] + 2.58 (7)

The methodology error was 1.33% ( Table 6 ). Although the error is within the limits of the equipment accuracy, ≤ 2%, there being no evidence of NBR low levels detection limit, the linearity is not as good as that found for the MIR, transmission and UATR methodologies.

3.6 NIRA analysis of NBR/SBR

To improve the results of NIR methodology, using the reflection method, the samples were analyzed by transflectance in this region (NIRA). The analytical bands chosen were the same. Figures 7 - 8 , Table 7 and Equation 8 shows the results obtained. The methodology error was 0.74% ( Table 7 ), with good linearity R = 0.96, and 92% of the data found were explained by this methodology. The error is within the limits of equipment accuracy, ≤ 2%, and there is no evidence of limit of detection of low levels of NBR.

Figure 7
NIRA Spectra (pyrolysis in Bunsen burner) of NBR/SBR blends.
Figure 8
NIRA calibration curve A4436/A4060 versus relative concentration [NBR/SBR].
Table 7
NIRA data (pyrolysis in Bunsen burner) for calibration curve elaboration and associated methodology errors.
A 4336 / A 4060 = 0.30 [ N B R ] / [ S B R ] + 2.46 (8)

To know the contents of unknown samples it is enough to analyze 5 aliquots of the rubber and to use the suitable calibration curves established in the developed methodologies, depending on the region of the infrared available in the laboratory. For example, Table 8 shows the evaluation of the MIR methodologies developed by means of analysis of unknown concentration NBR / SBR sample.

Table 8
Data of unknown NBR/SBR sample (X/Y) for validation of MIR methodologies developed.

Although the test sample has been analyzed by the analyst, without the knowledge of its concentration, the nominal value that should have been found would be around NBR70 / SBR30. Thus, both methodologies presented satisfactory values, with the best result for which UATR was used.

4. Conclusion

Summarily, all MIR and NIR methodologies were useful for NBR and SBR contents determination in the analyzed blends. The best correlation in the MIR region was found for the UATR methodology (pyrolysis in Bunsen burner), although there may be a detection limit between 10-20% NBR and an error around 3%. In the NIR region, the NIRA methodology showed better correlation, with no limit of detection and with error around 1%, within the limits of the FT-IR spectrometer. Both methodologies MIR/NIR are fast, therefore useful as quality control in different industrial and research scenarios.

5. Acknowledgements

This study was supported in part by the National Senior Visiting Professor Program (PVNS) from the Coordenação de Aperfeiçoamento Pessoal de Nível Superior (CAPES).

6. References

  • 1
    Hemais, C. A., Rosa, E. O. R., & Barros, H. M. (2000). Observações sobre desenvolvimentos Tecnológicos e os ciclos da Industria de Polímeros do Brasil. Polímeros: Ciência e Tecnologia, 10(3), 149-154. http://dx.doi.org/10.1590/S0104-14282000000300011.
    » http://dx.doi.org/10.1590/S0104-14282000000300011
  • 2
    Simielli, E. R. (1993). Principais características das blendas poliméricas fabricadas no Brasil. Polímeros: Ciência e Tecnologia , 3(1), 45-49. Retrieved in 2018, January 12, from http://www.revistapolimeros.org.br/pdf/v3n1/v3n1a06.pdf
    » http://www.revistapolimeros.org.br/pdf/v3n1/v3n1a06.pdf
  • 3
    Ramesan, M. T., Kuriakose, B., Pradeep, P., Alex, R., & Varghese, S. (2001). Compatibilization of SBR/NBR blends using chemically modified styrene butadiene rubber. International Polymer Processing, 16(2), 183-191. http://dx.doi.org/10.3139/217.1640.
    » http://dx.doi.org/10.3139/217.1640
  • 4
    Alcantara, A. F., Nunes, R. C. R., & Visconte, L. L. Y. (2004). Mistura BR/SBR: propriedades mecânicas em função de modo de preparo. Polímeros: Ciência e Tecnologia, 14(4), 279-282. http://dx.doi.org/10.1590/S0104-14282004000400015.
    » http://dx.doi.org/10.1590/S0104-14282004000400015
  • 5
    Rocha, T. C. J., Soares, B. G., & Coutinho, F. M. B. (2007). Principais copolímeros elastoméricos à base de butadieno utilizados na indústria automobilística. Polímeros: Ciência e Tecnologia, 17(4), 299-307. http://dx.doi.org/10.1590/S0104-14282007000400009.
    » http://dx.doi.org/10.1590/S0104-14282007000400009
  • 6
    Ramesan, M. T., & Alex, R. (2001). Compatibilization of SBR/NBR blends using chemically modified styrene-co-butadiene rubber - Part 2. Effect of compatibilizer loading. Polymer International, 50(12), 1298-1308. http://dx.doi.org/10.1002/pi.775.
    » http://dx.doi.org/10.1002/pi.775
  • 7
    Pedreira, S. M., Pinto, J. R. A., Campos, E. A., Mattos, E. D. C., Oliveira, M. S., Jr., Oliveira, J. I. S., & Dutra, R. D. C. L. (2016). Methodologies for characterization of aerospace polymers/energetic materials – a short review. Journal of Aerospace Technology and Management, 8(1), 18-25. http://dx.doi.org/10.5028/jatm.v8i1.576.
    » http://dx.doi.org/10.5028/jatm.v8i1.576
  • 8
    Wikipedia. (2018). Nitrile rubber Retrieved in 2018, January 12, from https://en.wikipedia.org/wiki/Nitrile_rubber
    » https://en.wikipedia.org/wiki/Nitrile_rubber
  • 9
    Sanches, N. B., Diniz, M. F., Alves, L. C., Dutra, J. C. N., Cassu, S. N., Azevedo, M. F. P., Mattos, E. C., & Dutra, R. C. L. (2008). Avaliação da aplicabilidade de técnicas FT-IR de reflexão (UATR) e de transmissão para a determinação do teor de acrilonitrila (AN) em NBR. Polímeros: Ciência e Tecnologia , 18(3), 249-255. http://dx.doi.org/10.1590/S0104-14282008000300011.
    » http://dx.doi.org/10.1590/S0104-14282008000300011
  • 10
    Chakraborty, S., Bandyopadhyay, S., Ameta, R., Mukhopadhyay, R., & Deuri, A. S. (2007). Application of FTIR in characterization of acrylonitrile-butadiene rubber (nitrile rubber). Polymer Testing, 26(1), 38-41. http://dx.doi.org/10.1016/j.polymertesting.2006.08.004.
    » http://dx.doi.org/10.1016/j.polymertesting.2006.08.004
  • 11
    Ghebremeskel, G. N., Sekinger, J. K., Hoffpauir, J. L., & Hendrix, C. (1996). A study on the thermal degradation products of styrene-butadiene type rubber by pyrolysis/GC/MS. Rubber Chemistry and Technology, 69(5), 874-884. http://dx.doi.org/10.5254/1.3538409.
    » http://dx.doi.org/10.5254/1.3538409
  • 12
    Yehia, A. A., Mansour, A. A., & Stoll, B. (1997). Detection of compatibility of some rubber blends by DSC. Journal of Thermal Analysis, 48(6), 1299-1310. http://dx.doi.org/10.1007/BF01983440.
    » http://dx.doi.org/10.1007/BF01983440
  • 13
    Ferreira, A. C., Diniz, M. F., & Mattos, E. C. (2018). FT-IR methodology transmission and UATR for quantifying automotive systems. Polímeros: Ciência e Tecnologia, 28(1), 6-14. http://dx.doi.org/10.1590/0104-1428.2412.
    » http://dx.doi.org/10.1590/0104-1428.2412
  • 14
    Choi, S.-S., Kim, Y., & Kwon, H.-M. (2014). Microstructural analysis and cis–transisomerization of BR and SBR vulcanizates reinforced with silica and carbon black using NMR and IR. RSC Advances, 4(59), 31113-31119. http://dx.doi.org/10.1039/C4RA03682D.
    » http://dx.doi.org/10.1039/C4RA03682D
  • 15
    Perez, L. D., & Lopez, B. L. (2012). Thermal characterization of SBR/NBR blends reinforced with a mesoporous silica. Journal of Applied Polymer Science, 125(S1), E327-E333. http://dx.doi.org/10.1002/app.35689.
    » http://dx.doi.org/10.1002/app.35689
  • 16
    Noriman, N. Z., Ismail, H., & Rashid, A. A. (2010). Characterization of styrene butadiene rubber/recycled acrylonitrile-butadiene rubber (SBR/NBRr) blends: The effects of epoxidized natural rubber (ENR-50) as a compatibilizer. Polymer Testing, 29(2), 200-208. http://dx.doi.org/10.1016/j.polymertesting.2009.11.002.
    » http://dx.doi.org/10.1016/j.polymertesting.2009.11.002
  • 17
    Dutra, R. C. L., Diniz, M. F., Ribeiro, A. P., Lourenço, V. L., Cassu, S. N., & Azevedo, M. P. (2004). Determinação do teor de NR/SBR em misturas: associação de dados DTG e FT-IR e/ou ensaios auxiliares. Polímeros: Ciência e Tecnologia, 14(5), 334-338. http://dx.doi.org/10.1590/S0104-14282004000500011.
    » http://dx.doi.org/10.1590/S0104-14282004000500011
  • 18
    Shield, S. R., Ghebremeskel, G. N., & Hendrix, C. (2001). Pyrolysis-GC/MS and TGA as tools for characterizing blends of SBR and NBR. Rubber Chemistry and Technology , 74(5), 803-813. http://dx.doi.org/10.5254/1.3547654.
    » http://dx.doi.org/10.5254/1.3547654
  • 19
    Shield, S. R., & Ghebremeskel, G. M. (2003). Use of mid and near infrared techniques as tools for characterizing blends of copolymers of styrene–butadiene and acrylonitrile-butadiene. Journal of Applied Polymer Science, 88(7), 1653-1658. http://dx.doi.org/10.1002/app.11849.
    » http://dx.doi.org/10.1002/app.11849
  • 20
    Fernández-Berridi, M. J., González, N., Mugica, A., & Bernicot, C. (2006). Pyrolysis-FTIR and TGA techniques as tools in the characterization of blends of natural rubber and SBR. Thermochimica Acta, 444(1), 65-70. http://dx.doi.org/10.1016/j.tca.2006.02.027.
    » http://dx.doi.org/10.1016/j.tca.2006.02.027
  • 21
    Lee, S. Y., Lee, W., Cho, S., Kim, I., & Ha, C. (2007). Quantitative analysis of unknown compositions in ternary polymer blends: a model study on NR/SBR/BR system. Journal of Analytical and Applied Pyrolysis, 78(1), 85-94. http://dx.doi.org/10.1016/j.jaap.2006.05.001.
    » http://dx.doi.org/10.1016/j.jaap.2006.05.001
  • 22
    Harada, M. (2015). Analytical methods for vulcanized rubbers. Nippon Gomu Kyokaishi , 88(6), 192-197. http://dx.doi.org/10.2324/gomu.88.192.
    » http://dx.doi.org/10.2324/gomu.88.192
  • 23
    Ujianto, O., Putri, D. B., Jayatin, & AWinarto, D. (2017). A comparative study of ground tire rubber devulcanization using twin screw extruder and internal mixer. IOP Conference Series. Materials Science and Engineering, 223, 012005. http://dx.doi.org/10.1088/1757-899X/223/1/012005.
    » http://dx.doi.org/10.1088/1757-899X/223/1/012005
  • 24
    Datta, S., Antos, J., & Stocek, R. (2017). Characterisation of ground tyre rubber by using combination of FT-IR numerical parameter and DTG analysis to determine the composition of ternary rubber blend. Polymer Testing, 59, 308-315. http://dx.doi.org/10.1016/j.polymertesting.2017.02.019.
    » http://dx.doi.org/10.1016/j.polymertesting.2017.02.019
  • 25
    Wake, W. C., Tidd, B. K., & Loadman, M. J. R. (1983). Analysis of rubber and rubber-like polymer 3rd ed. New York: Applied Science.
  • 26
    Rigoli, P. S., Murakami, L. M. S., Diniz, M. F., Azevedo, M. F. P., Cassu, S. N., Mattos, E. C., & Dutra, R. C. L. (In press). Quantification of aerospace polymer blends by thermogravimetric analysis and infrared spectrometry. Journal of Aerospace Technology and Management .
  • 27
    Goddu, R. F. (1960). Near-infrared spectrophotometry. In C. N. Reilly (Ed.), Advances in analytical chemistry and instrumentation (pp. 347-425). New York: Interscience.
  • 28
    Mello, T. S. D., Diniz, M. F., & Dutra, R. C. L. (2018). UATR and NIRA evaluation in the quantification of ATBC in NC blends. Polímeros: Ciência e Tecnologia , 28(3), 239-245. http://dx.doi.org/10.1590/0104-1428.16816.
    » http://dx.doi.org/10.1590/0104-1428.16816
  • 29
    Horák, V. M., & Vítek, A. (1978). Interpretation and processing of vibrational spectra New York: John Wiley & Sons.
  • 30
    Damazio, D., Santos, R. P., Diniz, M. F., & Dutra, R. C. L. (2015). Determinação do teor de ENB em EPDM (elastômero puro) por FT-IR de transmissão, por meio de banda relativa. Polímeros: Ciência e Tecnologia, 25(2), 181-185. http://dx.doi.org/10.1590/0104-1428.1777.
    » http://dx.doi.org/10.1590/0104-1428.1777
  • 31
    Grison, E. C., Becker, E., & Sartori, E. (2010). Borrachas e seus aditivos, componentes, influências e segredos. Porto Alegre: Letra e Vida.
  • 32
    Smith, A. L. (1979). Applied infrared spectroscopy New York: John Wiley & Sons.

Publication Dates

  • Publication in this collection
    29 Nov 2018
  • Date of issue
    Oct-Dec 2018

History

  • Received
    01 Feb 2018
  • Reviewed
    22 May 2018
  • Accepted
    20 June 2018
Associação Brasileira de Polímeros Rua São Paulo, 994, Caixa postal 490, São Carlos-SP, Tel./Fax: +55 16 3374-3949 - São Carlos - SP - Brazil
E-mail: revista@abpol.org.br