Photodegradation and Photostabilization of Poly(3-Hydroxybutyrate)

Abstract

The present work is concerned with the photodegradation and photostabilization of poly(3-hydroxybutyrate) (PHB) biopolymer. Two commercial grades of PHB were investigated, containing of 4.0% and 6.2% of hydroxyvalerate (HV) comonomer, named PHB1 and PHB2, respectively. Injection moulded specimens were exposed to ultraviolet radiation (UV-A) in the laboratory for periods of up to 12 weeks and then characterized by tensile testing, surface appearance, size exclusion chromatography (SEC), and scanning electron microscopy (SEM). The exposure to UV radiation caused great damaged on the surface color, reduction of molecular size and mechanical properties. The effects were more pronounced on PHB2, probably due a lighter surface color and less packed macromolecular structure which facilitates the transmission of light throughout the samples. Specimens of PHB1 were also injected with the addition of a UV absorber and antioxidant, resulting in a higher UV stability of PHB, as shown by a low reduction in molar mass and better mechanical properties.

Keywords
Biodegradable polymers; PHB; ultraviolet radiation; photodegradation; photostabilization


1. Introduction

Considering that the plastic-made products are in the center of many debates related to environmental issues, a current trend of the polymer community is the study of ways to reduce the environmental impact of these products11 Renstad R, Karlsson S, Albertsson AC, Werner PE, Westdahl M. Influence of Processing Parameters on the Mass Crystallinity of Poly(3-hydroxybutyrate- co-3-hydroxyvalerate). Polymer International. 1997;43(3):201-209. DOI: http://dx.doi.org/10.1002/(SICI)1097-0126(199707)43:3<201::AID-PI761>3.0.CO;2-7
http://dx.doi.org/10.1002/(SICI)1097-012...

2 Reddy K, Ghai R, Kalia C. Polyhydroxyalkanoates: an overview. Bioresource Technology. 2003; 87(2):137-146. DOI: http://dx.doi.org/10.1016/S0960-8524(02)00212-2
http://dx.doi.org/10.1016/S0960-8524(02)...

3 Cimmino S, Iodice P, Martuscelli E, Silvestre C. Poly(3-D(-)hydroxybutyrate)/atactic poly(methylmethacrylate) blends: Morphology, miscibility and crystallization relationships. Thermochimica Acta. 1998;321(1-2):89-98. DOI: http://dx.doi.org/10.1016/S0040-6031(98)00444-4
http://dx.doi.org/10.1016/S0040-6031(98)...

4 El-Hadi A, Schnabel R, Straube E, Müller G, Henning S. Correlation between degree of crystallinity, morphology, glass temperature, mechanical properties and biodegradation of poly (3-hydroxyalkanoate) PHAs and their blends. Polymer Testing. 2002;21(6):665-674. DOI: http://dx.doi.org/10.1016/S0142-9418(01)00142-8
http://dx.doi.org/10.1016/S0142-9418(01)...
-55 Bucci DZ, Tavares LBB, Sell I. PHB packaging for the storage of food products. Polymer Testing. 2005;24(5):564-571. DOI: http://dx.doi.org/10.1016/j.polymertesting.2005.02.008
http://dx.doi.org/10.1016/j.polymertesti...
. Besides the development of materials with a better recyclability, the use of biodegradable polymers and plastics obtained from renewable sources are some of the main objectives to achieve this goal. Committed to this purpose, we have been investigating the poly (3-hydroxybutyrate) (PHB) which is a natural and aliphatic polyester obtained from renewable sources. Our works have been focused on its phase transformation, crystallization and melting, stress cracking, mechanical, thermal and optical properties66 Wellen RMR, Rabello MS, Araújo Júnior IC, Fechine GJM, Canedo EL. Melting and crystallization of poly(3-hydroxybutyrate): effect of heating/cooling rates on phase transformation. Polímeros. 2015;25(3):296-304. DOI: http://dx.doi.org/10.1590/0104-1428.1961
http://dx.doi.org/10.1590/0104-1428.1961...

7 Wellen RMR, Rabello MS, Fechine GJM, Canedo EL. The melting behavior of poly(3-hydroxybutyrate) by DSC. Reproducibility study. Polymer Testing. 2015;32(2):215-220. DOI: http://dx.doi.org/10.1016/j.polymertesting.2012.11.001
http://dx.doi.org/10.1016/j.polymertesti...

8 Wellen RMR, Canedo EL, Lima CAV, Araújo Júnior IC, Almeida YMB, Rabello MS. The Effect of Polystyrene on the Crystallization of Poly(3-hydroxybutyrate). Materials Research. 2015;18(2):235-239. DOI: http://dx.doi.org/10.1590/1516-1439.242213
http://dx.doi.org/10.1590/1516-1439.2422...
-99 Wellen RMR, Rabello MS, Canedo EL. Melting and crystallization of poly(3-hydroxybutyrate)/carbon black compounds. Effect of heating and cooling cycles on phase transition. Journal of Materials Research. 2015;30(21):3211-3226. DOI: http://dx.doi.org/10.1557/jmr.2015.287
http://dx.doi.org/10.1557/jmr.2015.287...
. PHB used in the present work was produced from sugar cane plants, and was synthesized by biotechnological processes (microbial fermentation) without environmental damages.

PHB is inherently a non-toxic material and it is considered biocompatible, being used in medical applications like prosthesis, suture threats and devices for drugs release inside the human body1010 Farias RF, Canedo EL, Wellen RMR, Rabello MS. Environmental Stress Cracking of Poly(3-hydroxibutyrate) Under Contact with Sodium Hydroxide. Materials Research. 2015;18(2):258-266. DOI: http://dx.doi.org/10.1590/1516-1439.286114
http://dx.doi.org/10.1590/1516-1439.2861...
-1111 Carlo EC, Borges APB, Pompermayer LG, Martinez MMM, Eleotério RB, Nehme RC, et al. Composite for the fabrication of resorbable implants for osteosynthesis: biocompatibility evaluation in rabbits. Ciência Rural. 2009;39(1):135-140. DOI: http://dx.doi.org/10.1590/S0103-84782008005000036
http://dx.doi.org/10.1590/S0103-84782008...
. The general uses of PHB in replacement of ordinary plastics are growing, including applications like packing and other short life products like cups and cutleries for fast food restaurants. Due to its biodegradability, when discarded PHB can be attacked by microorganisms such as bacteria, and fungus which might be able to destroy its macromolecular chains producing CO2, CH4, H2O and microcellular organisms. These components return to the environment and could be used in another PHB's synthesis, in a typical life cycle of PHB. These characteristics make PHB a very promising material and efforts on establishing its properties, extending its applications, and optimizing its processing conditions are reported in the literature1212 Chen GQ, Wu Q. The application of polyhydroxyalkanoates as tissue engineering materials. Biomaterials. 2005;26(33):6565-6578. DOI: http://dx.doi.org/10.1016/j.biomaterials.2005.04.036
http://dx.doi.org/10.1016/j.biomaterials...

13 Modi S, Koelling K, Vodovotz Y. Assessment of PHB with varying hydroxyvalerate content for potential packaging applications. European Polymer Journal. 2011;47(2):179-186. DOI: http://dx.doi.org/10.1016/j.eurpolymj.2010.11.010
http://dx.doi.org/10.1016/j.eurpolymj.20...

14 Bahari K, Mitomo H, Enjoji T, Yoshii F, Makuuchi K. Degradability of poly(3-hydroxybutyrate) and its copolymer grafted with styrene by radiation. Polymer Degradation and Stability. 1998;61(2):245-252. DOI: http://dx.doi.org/10.1016/S0141-3910(97)00147-X
http://dx.doi.org/10.1016/S0141-3910(97)...

15 Harding KG, Dennis JS, von Blottnitz H, Harrison ST. Environmental analysis of plastic production processes: comparing petroleum-based polypropylene and polyethylene with biologically-based poly-beta-hydroxybutyric acid using life cycle analysis. Journal of Biotechnology. 2007;130(1):57-66. PMID: 17400318
-1616 Rhim J, Park HM, Ha CS. Bio-nanocomposites for food packaging applications. Progress in Polymer Science. 2013;38(10-11):1629-1652. DOI: http://dx.doi.org/10.1016/j.progpolymsci.2013.05.008
http://dx.doi.org/10.1016/j.progpolymsci...
.

Among the several possibilities of PHB application, we foresee the production of longer life consumer products. This assumption is based on the fact that the mechanical properties of this polymer are similar to usual polymers like polystyrene or polypropylene. If the product is not used or stored under conditions to withstand biodegradation, the lifetime could be compatible to the aimed application. Under this situation, the product can be exposed to ultraviolet radiation and, like the other types of polymers, suffer from this weathering condition. The photodegradation behavior of PHB, and the stabilization strategies, is scarcely reported in the literature1717 Sadi RK, Fechine GJM, Demarquette NR. Photodegradation of poly(3-hydroxybutyrate). Polymer Degradation and Stability. 2010; 95(12):2318-2327. DOI: http://dx.doi.org/10.1016/j.polymdegradstab.2010.09.003
http://dx.doi.org/10.1016/j.polymdegrads...
. The main objective of this work is to investigate the effects of ultraviolet radiation on PHB with different contents of hydroxyvalerate (HV) comonomers. Injection moulded specimens were exposed to weathering cycles of UV radiation, temperature and condensed water (humidity). The exposure procedure followed ASTM G-155 to simulate day (UV lights on) and night (UV lights off with water condensation)1818 Sadi RK, Fechine GJM, Demarquette NR. Effect of prior photodegradation on the biodegradation of polypropylene/poly(3-hydroxybutyrate) blends. Polymer Engineering & Science. 2013;53(10):2109-2122. DOI: http://dx.doi.org/10.1002/pen.23471
http://dx.doi.org/10.1002/pen.23471...
,1919 Fernandes LL, Freitas CA, Demarquette NR, Fechine GJM. Photodegradation of thermodegraded polypropylene/high-impact polystyrene blends: Mechanical properties. Journal of Applied Polymer Science. 2011;120(2):770-779. DOI: http://dx.doi.org/10.1002/app.33096
http://dx.doi.org/10.1002/app.33096...
. The effect of exposure was analyzed by scanning electron microscopy (SEM), tensile tests, and molecular weight. The use of stabilizing additives was also investigated.

2. Experimental

2.1. Materials and specimen preparation

Two random copolymers of 3-hydroxybutyrate (HB) with different contents of 3-hydroxyvalerate (HV) were used in the present study, both supplied by PHB Industrial SA (Brazil):

  • - FE-141, with 4% of HV, melt flow rate MFR 23-25 dg/min (ASTM D1238, 190ºC/2.16 kg), and number average molar weight Mn 52 kg/mol.

  • - FE-112 with 6.2% of HV, MFR 30-33 dg/min (ASTM D1238, 190ºC/2.16 kg), Mn 76.2 kg/mol.

The resins were coded as PHB1 and PHB2, respectively. In an attempt to evaluate the effect of stabilizing additives, a UV absorber Tinuvin 791FB (0.25%) and an antioxidant Irganox B215 (0.40%) were added to PHB1; this material was coded PHBABS. The amount of additives was chosen based on manufacturer´s recommendation. The chemicals structures of HB and HV units are shown in Figure 1.

Figure 1
Structural units of 3-hydroxybutyrate HB (a) and 3-hydroxyvalerate HV (b).

Type I (ASTM D-638) tensile test specimen of PHB1, PHB2 and PHBABS were produced in a Romi 130 injection molding machine, operating with barrel temperature ranging between 150-190ºC and the mold at 20ºC.

2.2. Methods

The exposure to ultraviolet (UV) radiation was done with the tensile tests specimens for up to 12 weeks in an accelerated weathering chamber Q-Lab, type QUV, containing UV-A fluorescent tubes. These lamps have a maximum irradiance of 0.89 W/m22 Reddy K, Ghai R, Kalia C. Polyhydroxyalkanoates: an overview. Bioresource Technology. 2003; 87(2):137-146. DOI: http://dx.doi.org/10.1016/S0960-8524(02)00212-2
http://dx.doi.org/10.1016/S0960-8524(02)...
at 340 nm. The weathering cycles were: 8 hours under UV light at 60ºC and 4 hours in the dark under condensed water at 50ºC. The exposure procedure carried out according to ASTM G-155.

Molecular weight analyses were conducted by size exclusion chromatography (SEC) using a Viscotek HT-GPC equipment at 40ºC with a refractive index detector. Samples used for SEC analysis were removed from the surface (up to 1 mm) of the tensile test specimen directly exposed to UV radiation. The polymer was dissolved in chloroform and the filtered solution was injected into the equipment. The solvent flow rate was 1 mL/min and the columns were calibrated with narrow molecular weight PS.

Mechanical tests were done in accordance to ASTM D638 at 20 mm/min at 23ºC, using an EMIC model DL2000 universal testing machine with load cell of 5 kN. The results reported represent averages of at least four test samples.

Scanning electron microscopy images of fractured surface were taken in a JEOL 6460, the samples were cryogenically fractured in liquid nitrogen and covered with carbon to avoid the charge accumulation.

The crystallinity degree of the exposed surface of samples was obtained by X-ray diffraction in a Rigaku-Dairix Miniflex II equipment using Cu Kα radiation (1.54 Å), and a scattering angles range of 2θ = 4-90° at a rate of 3°/min.

3. Results and Discussion

Photographs of PHB1 and PHB2 sample tests unexposed and exposed to UV radiation for 6 and 12 weeks are showed in Figure 2. The exposed surfaces, previously brown and caramel, turned into caramel and whitish, respectively, after 12 weeks under UV exposure. According to previous works done by one of the current authors1717 Sadi RK, Fechine GJM, Demarquette NR. Photodegradation of poly(3-hydroxybutyrate). Polymer Degradation and Stability. 2010; 95(12):2318-2327. DOI: http://dx.doi.org/10.1016/j.polymdegradstab.2010.09.003
http://dx.doi.org/10.1016/j.polymdegrads...
,1818 Sadi RK, Fechine GJM, Demarquette NR. Effect of prior photodegradation on the biodegradation of polypropylene/poly(3-hydroxybutyrate) blends. Polymer Engineering & Science. 2013;53(10):2109-2122. DOI: http://dx.doi.org/10.1002/pen.23471
http://dx.doi.org/10.1002/pen.23471...
, this whitening does not result from the formation of chromophoric groups, but it is probably originated from a topological feature of the UV exposed samples, where cracks are formed on PHB1 and PHB2 surfaces. The occurrence of surface cracking was previously associated with polypropylene whitening during UV exposure1717 Sadi RK, Fechine GJM, Demarquette NR. Photodegradation of poly(3-hydroxybutyrate). Polymer Degradation and Stability. 2010; 95(12):2318-2327. DOI: http://dx.doi.org/10.1016/j.polymdegradstab.2010.09.003
http://dx.doi.org/10.1016/j.polymdegrads...
, in which the cracks increase the roughness of the surface, raising the diffuse reflectance of the visible light.

Figure 2
Photographs of PHB1 and PHB2 tests specimens illustrating samples whitening under UV exposure. Exposing time (weeks) indicated.

The results of tensile tests for PHB1 and PHB2 unexposed and exposed up to 12 weeks are presented in Table 1, together with the results of molar mass determination. The average scissions number (SN) per macromolecule presented in Table 1 was determined using Equation 1:

SN = M no M nt Eq . 1

Table 1
Mechanical properties and Mn of PHB1 and PHB2 before and after exposure to UV radiation.

Where: Mno and Mnt are the number-average molecular weight of the material unexposed and exposed to UV radiation for a given time, respectively.

Tensile strength and strain at break reduced with exposure time. After 12 weeks of severe weathering conditions of UV, temperature and condensed water, the tensile strength of PHB1 and PHB2 decreased 32% and 34%, the strain at break decreased 30% and 42%, respectively. According to work reported elsewhere1717 Sadi RK, Fechine GJM, Demarquette NR. Photodegradation of poly(3-hydroxybutyrate). Polymer Degradation and Stability. 2010; 95(12):2318-2327. DOI: http://dx.doi.org/10.1016/j.polymdegradstab.2010.09.003
http://dx.doi.org/10.1016/j.polymdegrads...
when PHB is under UV radiation, two mechanisms might occur in parallel, i.e., macromolecular crosslinking and chain scission; one of them will be dominant and may be visualized by the change in number-average molecular weight (Mn). Concerning the results showed in Table 1, Mn values of PHB1 and PHB2 decreased upon UV exposure, hence it can be deduced that the macromolecular scission is the preponderant mechanism observed here and that this is the main reason for the reduction in tensile properties.

The HV content should be considered influencing the photodegradation of PHB. Since the HV unit is bulkier than the HB unit (see Figure 1), we have an expectation that the copolymer with a higher HV content (PHB2) would be more susceptible to the degradation effects due to a higher free volume and hence a higher diffusion of oxygen and moisture. Commonly, PHB suffer degradation also by hydrolysis mechanisms1717 Sadi RK, Fechine GJM, Demarquette NR. Photodegradation of poly(3-hydroxybutyrate). Polymer Degradation and Stability. 2010; 95(12):2318-2327. DOI: http://dx.doi.org/10.1016/j.polymdegradstab.2010.09.003
http://dx.doi.org/10.1016/j.polymdegrads...

18 Sadi RK, Fechine GJM, Demarquette NR. Effect of prior photodegradation on the biodegradation of polypropylene/poly(3-hydroxybutyrate) blends. Polymer Engineering & Science. 2013;53(10):2109-2122. DOI: http://dx.doi.org/10.1002/pen.23471
http://dx.doi.org/10.1002/pen.23471...

19 Fernandes LL, Freitas CA, Demarquette NR, Fechine GJM. Photodegradation of thermodegraded polypropylene/high-impact polystyrene blends: Mechanical properties. Journal of Applied Polymer Science. 2011;120(2):770-779. DOI: http://dx.doi.org/10.1002/app.33096
http://dx.doi.org/10.1002/app.33096...

20 Rabello MS, White JR. Crystallization and melting behaviour of photodegraded polypropylene - I. Chemi-crystallization. Polymer. 1997;38(26):6379-6387. DOI: http://dx.doi.org/10.1016/S0032-3861(97)00213-9
http://dx.doi.org/10.1016/S0032-3861(97)...
-2121 Freier T, Kunze C, Nischan C, Kramer S, Sternberg K, Saß M, et al. In vitro and in vivo degradation studies for development of a biodegradable patchbased on poly(3-hydroxybutyrate). Biomaterials. 2002;23(13):2649-2657. PMID: 12059014 DOI: http://dx.doi.org/10.1016/S0142-9612(01)00405-7
http://dx.doi.org/10.1016/S0142-9612(01)...
, i.e., under humidity environment and temperature, chain scission occurs and, together with the photodegradation effects, will contribute to the deterioration in the polymer properties. If the specimen has a more open structure as it is in PHB2 the effects of UV radiation, humidity and temperature may be more severe - as was observed for PHB2 specimens in Figure 2, and serious damage are usually observed in the mechanical properties, as shown in Table 1. Another effect is that samples with higher content of HV is lighter and, as a consequence, the UV radiation can reach deeper regions comparing with the darker samples with low content of HV.

Scanning electron microscopy (SEM) images of PHB1 and PHB2 surfaces photodegraded up to 12 weeks are presented on Figure 3. As can be seen in this Figure, the sample PHB1 did not show any significant changes at the surface; however; sample PHB2 presented cracks after 6 weeks of exposure and the density of the cracks increased with the exposure time. As presented before, the drop in mechanical properties was more intense for PHB2; the presence of cracks on the surface of these samples is a major reason for this behavior. The cracks formed during exposure are usually related to an increase on surface crystallinity, a phenomenon called chemi-crystallization that occurs due to rearrangement of taut molecules that are released by the chain scission events2020 Rabello MS, White JR. Crystallization and melting behaviour of photodegraded polypropylene - I. Chemi-crystallization. Polymer. 1997;38(26):6379-6387. DOI: http://dx.doi.org/10.1016/S0032-3861(97)00213-9
http://dx.doi.org/10.1016/S0032-3861(97)...
.

Figure 3
Scanning electron microscopy (SEM) images of PHB1 non-exposed (a) and exposed for 3 (b), 6 (c) and 12 weeks (d); and PHB2 non-exposed (e) and exposed for 3 (f), 6 (g) and 12 weeks (h).

Scanning electron microscopy (SEM) images of fractured surface of PHB1 and PHB2 photodegraded for 12 weeks are given in Figure 4. The fracture surface of PHB2 showed a smoother topography and similar size photodegraded zone when compared to PHB1. By SEM images it is showed an increase in photodegraded zone with exposure time. Similar trend like that observed for 12 weeks was seen in other samples, exposed for 3, 6 and 9 weeks (results not showed here) where PHB2 has larger photodegraded zones than PHB1.

Figure 4
SEM images of fractured surface of PHB1 (a) and PHB2 (b) exposed to UV radiation during 12 weeks. The arrows indicate the interface between the degraded and the not-degraded material. (PZ: Photodegradaded Zone)

In an attempt to protect PHB from UV effects, antioxidant and UV absorber additives were added to PHB and samples were exposed for up to 6 weeks under the same weathering conditions described before. The molecular weight distribution curves of PHB1 and PHBABS unexposed and exposed for different times are presented in Figure 5. It is clear that the molecular weight distribution curves for PHB1 showed a significant modification in peak location and shape as exposure time is increased. However, PHBABS did not present a major modification on the distribution curves. A consequence of this is observed on the polydispersity values (Mw/Mn). The polydispersity of PHB1 changes from 2.6 (unexposed) to 3.7 (6 weeks exposure), whereas PHBABS only changes from 2.2 to 2.6.

Figure 5
Molecular weight distribution curves of PHB1 (a) and PHBABS (b) not exposure and exposed for different times.

Table 2 presents the results of tensile tests, Mn and SN for PHB1 and PHBABS. It can be observed that the mechanical properties tend to a slight decrease with the exposure time for PHB1 whereas no significant changes could be seen for PHBABS. The molecular weight decreased as much as 77.5% after 6 weeks of exposure for PHB1. On the other hand, the reduction of Mn for PHBABS was 43.8% after 6 weeks. The chain scissions in PHBAbs were 58% and 44% lower than PHB1 for analyses taken at 3 and 6 weeks, respectively. The results indicate that the UV absorber and antioxidant additives protected the PHB matrix from the UV radiation1818 Sadi RK, Fechine GJM, Demarquette NR. Effect of prior photodegradation on the biodegradation of polypropylene/poly(3-hydroxybutyrate) blends. Polymer Engineering & Science. 2013;53(10):2109-2122. DOI: http://dx.doi.org/10.1002/pen.23471
http://dx.doi.org/10.1002/pen.23471...
,2121 Freier T, Kunze C, Nischan C, Kramer S, Sternberg K, Saß M, et al. In vitro and in vivo degradation studies for development of a biodegradable patchbased on poly(3-hydroxybutyrate). Biomaterials. 2002;23(13):2649-2657. PMID: 12059014 DOI: http://dx.doi.org/10.1016/S0142-9612(01)00405-7
http://dx.doi.org/10.1016/S0142-9612(01)...

22 Kasuya K, Inoue Y, Yamada K, Doi Y. Kinetics of surface hydrolysis of poly[(R)-3-hydroxybutyrate] film by PHB depolymerase from Alcaligenes faecalis Tl. Polymer Degradation and Stability. 1995;48(1):167-174. DOI: http://dx.doi.org/10.1016/0141-3910(95)00026-I
http://dx.doi.org/10.1016/0141-3910(95)0...

23 La Mantia FP. Recycling of heterogeneous plastics wastes. II - The role of modifier agents. Polymer Degradation and Stability. 1993;42(2):213-218. DOI: http://dx.doi.org/10.1016/0141-3910(93)90114-X
http://dx.doi.org/10.1016/0141-3910(93)9...
-2424 Parra DF, Fusaro J, Gaboardi F, Rosa DS. Influence of poly (ethylene glycol) on the thermal, mechanical, morphological, physical-chemical and biodegradation properties of poly (3-hydroxybutyrate). Polymer Degradation and Stability. 2006;91(9):1954-1959. DOI: http://dx.doi.org/10.1016/j.polymdegradstab.2006.02.008
http://dx.doi.org/10.1016/j.polymdegrads...
.

Table 2
Mechanical properties and of PHB and PHBABS before and after exposure to UV radiation for different times.

Table 3 shows the crystallinity degree (Xc) of the samples calculated by XRD before and after exposure to UV radiation. After three weeks PHB1, PHB2 and PHBABS presented an increasing on the Xc values followed by drop until 12 weeks. The first phenomenon is very known and called chemi-crystallization, it has been reported in the literature2020 Rabello MS, White JR. Crystallization and melting behaviour of photodegraded polypropylene - I. Chemi-crystallization. Polymer. 1997;38(26):6379-6387. DOI: http://dx.doi.org/10.1016/S0032-3861(97)00213-9
http://dx.doi.org/10.1016/S0032-3861(97)...
and usually takes place when polymers are exposed to UV radiation. The chemi-crystallization occurs with degraded molecules (decreased on molecular weight) rearrange themselves in the form of crystals. It could be happened because the temperature inside the UV chamber (50-60°C) was higher enough to allow the cold crystallization mechanisms to develop99 Wellen RMR, Rabello MS, Canedo EL. Melting and crystallization of poly(3-hydroxybutyrate)/carbon black compounds. Effect of heating and cooling cycles on phase transition. Journal of Materials Research. 2015;30(21):3211-3226. DOI: http://dx.doi.org/10.1557/jmr.2015.287
http://dx.doi.org/10.1557/jmr.2015.287...
. After longer periods of exposure, it is possible that the chain becomes too defective by the presence of groups containing oxygen and, hence, further organization may be more difficult2020 Rabello MS, White JR. Crystallization and melting behaviour of photodegraded polypropylene - I. Chemi-crystallization. Polymer. 1997;38(26):6379-6387. DOI: http://dx.doi.org/10.1016/S0032-3861(97)00213-9
http://dx.doi.org/10.1016/S0032-3861(97)...
. Destruction of crystals by the degradation effects has also been reported2525 Vaughan AS, Stevens GC. On radiation effects in poly(ethylene terephtalate): a comparison with poly(ether ether ketone). Polymer. 19953681541-1547http://dx.doi.org/10.1016/0032-3861(95)98997-2
http://dx.doi.org/10.1016/0032-3861(95)9...
. In the case of PHBABS the values of Xc increased until 6 weeks indicating that the level of the scissions was not enough to hindering the chemi-crystallization phenomenon. These results are consistent with molecular weight and mechanical properties, indicating that the UV absorber and antioxidant acted very well in PHB matrix.

Table 3
Crystallinity degree (Xc) of PHB1, PHB2 and PHBABS before and after exposure to UV radiation for different times.

4. Conclusion

The results presented in this work showed that there is a significant difference on the photodegradation damages of PHB depending on its HV content. This difference is not only due to the chemical structure but also to the color of the samples. The PHB with a higher HV content is lighter than the PHB with a lower HV content and, as consequence; the penetration of UV radiation is deeper into the test bars. The results after 12 weeks showed that whiteness, mechanical properties, molecular weight and fracture surface damages were more accentuated on PHB with higher HV content. The additions of the UV absorber and the antioxidant additives have improved the UV stability of PHB, with a significant reduction on the photodegradation rate, as observed by mechanical properties, molecular weight and crystallinity degree. It is hoped that these results could be useful to design materials with more stability during processing and ultraviolet exposure while maintaining their characteristic of biodegradability.

5. Acknowledgments

The authors wish to thank PHB Industrial SA (Brazil) for supplying the raw materials, to Prof. Agnelli (UFSCar, Brazil) for injection moulding PHBs sample tests, CNPq/Brazil (MCTI/CNPq Nº 14/2012 Process Number: 478124/2012-0) and FAPESP/SP/Brazil for the financial support. RMRW thanks to Eduardo Brondi from PHB Industrial SA (Brazil) for discussions related to this work.

6. References

  • 1
    Renstad R, Karlsson S, Albertsson AC, Werner PE, Westdahl M. Influence of Processing Parameters on the Mass Crystallinity of Poly(3-hydroxybutyrate- co-3-hydroxyvalerate). Polymer International 1997;43(3):201-209. DOI: http://dx.doi.org/10.1002/(SICI)1097-0126(199707)43:3<201::AID-PI761>3.0.CO;2-7
    » http://dx.doi.org/10.1002/(SICI)1097-0126(199707)43:3<201::AID-PI761>3.0.CO;2-7
  • 2
    Reddy K, Ghai R, Kalia C. Polyhydroxyalkanoates: an overview. Bioresource Technology 2003; 87(2):137-146. DOI: http://dx.doi.org/10.1016/S0960-8524(02)00212-2
    » http://dx.doi.org/10.1016/S0960-8524(02)00212-2
  • 3
    Cimmino S, Iodice P, Martuscelli E, Silvestre C. Poly(3-D(-)hydroxybutyrate)/atactic poly(methylmethacrylate) blends: Morphology, miscibility and crystallization relationships. Thermochimica Acta 1998;321(1-2):89-98. DOI: http://dx.doi.org/10.1016/S0040-6031(98)00444-4
    » http://dx.doi.org/10.1016/S0040-6031(98)00444-4
  • 4
    El-Hadi A, Schnabel R, Straube E, Müller G, Henning S. Correlation between degree of crystallinity, morphology, glass temperature, mechanical properties and biodegradation of poly (3-hydroxyalkanoate) PHAs and their blends. Polymer Testing 2002;21(6):665-674. DOI: http://dx.doi.org/10.1016/S0142-9418(01)00142-8
    » http://dx.doi.org/10.1016/S0142-9418(01)00142-8
  • 5
    Bucci DZ, Tavares LBB, Sell I. PHB packaging for the storage of food products. Polymer Testing 2005;24(5):564-571. DOI: http://dx.doi.org/10.1016/j.polymertesting.2005.02.008
    » http://dx.doi.org/10.1016/j.polymertesting.2005.02.008
  • 6
    Wellen RMR, Rabello MS, Araújo Júnior IC, Fechine GJM, Canedo EL. Melting and crystallization of poly(3-hydroxybutyrate): effect of heating/cooling rates on phase transformation. Polímeros 2015;25(3):296-304. DOI: http://dx.doi.org/10.1590/0104-1428.1961
    » http://dx.doi.org/10.1590/0104-1428.1961
  • 7
    Wellen RMR, Rabello MS, Fechine GJM, Canedo EL. The melting behavior of poly(3-hydroxybutyrate) by DSC. Reproducibility study. Polymer Testing 2015;32(2):215-220. DOI: http://dx.doi.org/10.1016/j.polymertesting.2012.11.001
    » http://dx.doi.org/10.1016/j.polymertesting.2012.11.001
  • 8
    Wellen RMR, Canedo EL, Lima CAV, Araújo Júnior IC, Almeida YMB, Rabello MS. The Effect of Polystyrene on the Crystallization of Poly(3-hydroxybutyrate). Materials Research 2015;18(2):235-239. DOI: http://dx.doi.org/10.1590/1516-1439.242213
    » http://dx.doi.org/10.1590/1516-1439.242213
  • 9
    Wellen RMR, Rabello MS, Canedo EL. Melting and crystallization of poly(3-hydroxybutyrate)/carbon black compounds. Effect of heating and cooling cycles on phase transition. Journal of Materials Research 2015;30(21):3211-3226. DOI: http://dx.doi.org/10.1557/jmr.2015.287
    » http://dx.doi.org/10.1557/jmr.2015.287
  • 10
    Farias RF, Canedo EL, Wellen RMR, Rabello MS. Environmental Stress Cracking of Poly(3-hydroxibutyrate) Under Contact with Sodium Hydroxide. Materials Research 2015;18(2):258-266. DOI: http://dx.doi.org/10.1590/1516-1439.286114
    » http://dx.doi.org/10.1590/1516-1439.286114
  • 11
    Carlo EC, Borges APB, Pompermayer LG, Martinez MMM, Eleotério RB, Nehme RC, et al. Composite for the fabrication of resorbable implants for osteosynthesis: biocompatibility evaluation in rabbits. Ciência Rural 2009;39(1):135-140. DOI: http://dx.doi.org/10.1590/S0103-84782008005000036
    » http://dx.doi.org/10.1590/S0103-84782008005000036
  • 12
    Chen GQ, Wu Q. The application of polyhydroxyalkanoates as tissue engineering materials. Biomaterials 2005;26(33):6565-6578. DOI: http://dx.doi.org/10.1016/j.biomaterials.2005.04.036
    » http://dx.doi.org/10.1016/j.biomaterials.2005.04.036
  • 13
    Modi S, Koelling K, Vodovotz Y. Assessment of PHB with varying hydroxyvalerate content for potential packaging applications. European Polymer Journal 2011;47(2):179-186. DOI: http://dx.doi.org/10.1016/j.eurpolymj.2010.11.010
    » http://dx.doi.org/10.1016/j.eurpolymj.2010.11.010
  • 14
    Bahari K, Mitomo H, Enjoji T, Yoshii F, Makuuchi K. Degradability of poly(3-hydroxybutyrate) and its copolymer grafted with styrene by radiation. Polymer Degradation and Stability 1998;61(2):245-252. DOI: http://dx.doi.org/10.1016/S0141-3910(97)00147-X
    » http://dx.doi.org/10.1016/S0141-3910(97)00147-X
  • 15
    Harding KG, Dennis JS, von Blottnitz H, Harrison ST. Environmental analysis of plastic production processes: comparing petroleum-based polypropylene and polyethylene with biologically-based poly-beta-hydroxybutyric acid using life cycle analysis. Journal of Biotechnology 2007;130(1):57-66. PMID: 17400318
  • 16
    Rhim J, Park HM, Ha CS. Bio-nanocomposites for food packaging applications. Progress in Polymer Science 2013;38(10-11):1629-1652. DOI: http://dx.doi.org/10.1016/j.progpolymsci.2013.05.008
    » http://dx.doi.org/10.1016/j.progpolymsci.2013.05.008
  • 17
    Sadi RK, Fechine GJM, Demarquette NR. Photodegradation of poly(3-hydroxybutyrate). Polymer Degradation and Stability 2010; 95(12):2318-2327. DOI: http://dx.doi.org/10.1016/j.polymdegradstab.2010.09.003
    » http://dx.doi.org/10.1016/j.polymdegradstab.2010.09.003
  • 18
    Sadi RK, Fechine GJM, Demarquette NR. Effect of prior photodegradation on the biodegradation of polypropylene/poly(3-hydroxybutyrate) blends. Polymer Engineering & Science 2013;53(10):2109-2122. DOI: http://dx.doi.org/10.1002/pen.23471
    » http://dx.doi.org/10.1002/pen.23471
  • 19
    Fernandes LL, Freitas CA, Demarquette NR, Fechine GJM. Photodegradation of thermodegraded polypropylene/high-impact polystyrene blends: Mechanical properties. Journal of Applied Polymer Science 2011;120(2):770-779. DOI: http://dx.doi.org/10.1002/app.33096
    » http://dx.doi.org/10.1002/app.33096
  • 20
    Rabello MS, White JR. Crystallization and melting behaviour of photodegraded polypropylene - I. Chemi-crystallization. Polymer 1997;38(26):6379-6387. DOI: http://dx.doi.org/10.1016/S0032-3861(97)00213-9
    » http://dx.doi.org/10.1016/S0032-3861(97)00213-9
  • 21
    Freier T, Kunze C, Nischan C, Kramer S, Sternberg K, Saß M, et al. In vitro and in vivo degradation studies for development of a biodegradable patchbased on poly(3-hydroxybutyrate). Biomaterials 2002;23(13):2649-2657. PMID: 12059014 DOI: http://dx.doi.org/10.1016/S0142-9612(01)00405-7
    » http://dx.doi.org/10.1016/S0142-9612(01)00405-7
  • 22
    Kasuya K, Inoue Y, Yamada K, Doi Y. Kinetics of surface hydrolysis of poly[(R)-3-hydroxybutyrate] film by PHB depolymerase from Alcaligenes faecalis Tl. Polymer Degradation and Stability 1995;48(1):167-174. DOI: http://dx.doi.org/10.1016/0141-3910(95)00026-I
    » http://dx.doi.org/10.1016/0141-3910(95)00026-I
  • 23
    La Mantia FP. Recycling of heterogeneous plastics wastes. II - The role of modifier agents. Polymer Degradation and Stability 1993;42(2):213-218. DOI: http://dx.doi.org/10.1016/0141-3910(93)90114-X
    » http://dx.doi.org/10.1016/0141-3910(93)90114-X
  • 24
    Parra DF, Fusaro J, Gaboardi F, Rosa DS. Influence of poly (ethylene glycol) on the thermal, mechanical, morphological, physical-chemical and biodegradation properties of poly (3-hydroxybutyrate). Polymer Degradation and Stability 2006;91(9):1954-1959. DOI: http://dx.doi.org/10.1016/j.polymdegradstab.2006.02.008
    » http://dx.doi.org/10.1016/j.polymdegradstab.2006.02.008
  • 25
    Vaughan AS, Stevens GC. On radiation effects in poly(ethylene terephtalate): a comparison with poly(ether ether ketone). Polymer 19953681541-1547http://dx.doi.org/10.1016/0032-3861(95)98997-2
    » http://dx.doi.org/10.1016/0032-3861(95)98997-2

Publication Dates

  • Publication in this collection
    13 May 2016
  • Date of issue
    Jul-Aug 2016

History

  • Received
    03 Nov 2015
  • Reviewed
    02 Mar 2016
  • Accepted
    26 Apr 2016
ABM, ABC, ABPol UFSCar - Dep. de Engenharia de Materiais, Rod. Washington Luiz, km 235, 13565-905 - São Carlos - SP- Brasil. Tel (55 16) 3351-9487 - São Carlos - SP - Brazil