Acessibilidade / Reportar erro

Cytotoxicity and genotoxicity of calcium silicate-based cements on an osteoblast lineage

Abstract

Several calcium silicate-based biomaterials have been developed in recent years, in addition to Mineral Trioxide Aggregate (MTA). The aim of this study was to evaluate the cytotoxicity, genotoxicity and apoptosis/necrosis in human osteoblast cells (SAOS-2) of pure calcium silicate-based cements (CSC) and modified formulations: modified calcium silicate-based cements (CSCM) and three resin-based calcium silicate cements (CSCR1) (CSCR 2) (CSCR3). The following tests were performed after 24 hours of cement extract exposure: methyl-thiazolyl tetrazolium (MTT), apoptosis/necrosis assay and comet assay. The negative control (CT-) was performed with untreated cells, and the positive control (CT+) used hydrogen peroxide. The data for MTT and apoptosis were submitted to analysis of variance and Bonferroni’s posttest (p < 0.05), and the data for the comet assay analysis, to the Kruskal-Wallis and Dunn tests (p < 0.05). The MTT test showed no significant difference among the materials in 2 mg/mL and 10 mg/mL concentrations. CSCR3 showed lower cell viability at 10 mg/mL. Only CSC showed lower cell viability at 50 mg/mL. CSCR1, CSCR2 and CSCR3 showed a higher percentage of initial apoptosis than the control in the apoptosis test, after 24 hours exposure. The same cements showed no genotoxicity in the concentration of 2 mg/mL, with the comet assay. CSC and CSCR2 were also not genotoxic at 10 mg/mL. All experimental materials showed viability with MTT. CSC and CSCR2 presented a better response to apoptosis and genotoxicity evaluation in the 10 mg/mL concentration, and demonstrated a considerable potential for use as reparative materials.

Cytotoxicity, Immunologic; Mutagenicity Tests; Calcium Compounds

Introduction

An innovative repair material was developed in 1993 at the University of Loma Linda, called Mineral Trioxide Aggregate (MTA).11. Torabinejad M, Watson TF, Pitt Ford TR. Sealing ability of a mineral trioxide aggregate when used as a root end filling material. J Endod. 1993;19(12):591-5. doi:10.1016/S0099-2399(06)80271-2
https://doi.org/10.1016/S0099-2399(06)80...
MTA has been used successfully for apexification, internal root resorption, endodontic surgery, sealing of perforations, and as a pulp-capping material.22. Torabinejad M, Parirokh M. Mineral trioxide aggregate: a comprehensive literature review - part II: leakage and biocompatibility investigations. J Endod. 2010 Feb;36(2):190-202. doi:10.1016/j.joen.2009.09.010
https://doi.org/10.1016/j.joen.2009.09.0...
Fine particles of tricalcium silicate, tricalcium aluminum, tricalcium oxide and other oxide materials, in addition to bismuth oxide, which promotes the radiopacity of cement, make up the composition of MTA powder, which sets on contact with water.33. Tanomaru-Filho M, Bosso R, Viapiana R, Guerreiro-Tanomaru JM. Radiopacity and flow of different endodontic sealers. Acta Odontol Latinoam. 2013;26(2):121-5. MTA is a non-cytotoxic reparative material with excellent biological properties.44. Pelliccioni GA, Ciapetti G, Cenni E, Granchi D, Nanni M, Pagani S, et al. Evaluation of osteoblast-like cell response to Proroot MTA (mineral trioxide aggregate) cement. J Mater Sci Mater Med. 2004;15(2):167-73. doi:10.1023/B:JMSM.0000011819.26935.47
https://doi.org/10.1023/B:JMSM.000001181...
MTA contributes to reducing inflammation and necrosis levels. The use of MTA as pulp-capping material induces the formation of a dentin bridge, allowing repair and pulp vitality.55. Bogen G, Kim JS, Bakland LK. Direct pulp capping with mineral trioxide aggregate: an observational study. J Am Dent Assoc. 2008;139(3):305-15; quiz 305-15. Erratum in: J Am Dent Assoc. 2008;139(5):541. Various studies have shown that the physicochemical and biological properties of MTA are similar to those of Portland Cement (PC), a calcium silicate-based cement (CSC).66. Oliveira MG, Xavier CB, Demarco FF, Pinheiro AL, Costa AT, Pozza DH. Comparative chemical study of MTA and Portland cements. Braz Dent J. 2007;18(1):3-7. doi:10.1590/S0103-64402007000100002
https://doi.org/10.1590/S0103-6440200700...
,77. Gonçalves JL, Viapiana R, Miranda CE, Borges AH, Cruz Filho AM. Evaluation of physico-chemical properties of Portland cements and MTA. Braz Oral Res. 2010;24(3):277-83. doi:10.1590/S1806-83242010000300004
https://doi.org/10.1590/S1806-8324201000...

Calcium silicate based cements (CSC) have the potential to stimulate cell proliferation and osteoblast-related gene expression in osteoblasts.88. Maeno S, Niki Y, Matsumoto H, Morioka H, Yatabe T, Funayama A, et al. The effect of calcium ion concentration on osteoblast viability, proliferation and differentiation in monolayer and 3D culture. Biomaterials. 2005;26(23):4847-55. doi:10.1016/j.biomaterials.2005.01.006
https://doi.org/10.1016/j.biomaterials.2...
,99. Sun J, Wei L, Liu X, Li J, Li B, Wang G, et al. Influences of ionic dissolution products of dicalcium silicate coating on osteoblastic proliferation, differentiation and gene expression. Acta Biomater. 2009;5(4):1284-93. doi:10.1016/j.actbio.2008.10.011
https://doi.org/10.1016/j.actbio.2008.10...
Anti-inflammatory effects and dentinogenic potential have been observed in primary pulp cells and mouse dental papilla cell-23 (MDPC-23) cells exposed to CSC cements, respectively.1010. Eid AA, Niu L-n, Primus CM, Opperman LA, Watanabe I, Pashley DH, et al. In vitro osteogenic/dentinogenic potential of an experimental calcium aluminosilicate cement. J Endod. 2013;39(9):1161-6. doi:10.1016/j.joen.2013.04.005
https://doi.org/10.1016/j.joen.2013.04.0...
,1111. Chen CL, Kao CT, Ding SJ, Shie MY, Huang TH. Expression of the inflammatory marker cyclooxygenase-2 in dental pulp cells cultured with mineral trioxide aggregate or calcium silicate cements. J Endod. 2010;36(3):465-8. doi:10.1016/j.joen.2009.12.008
https://doi.org/10.1016/j.joen.2009.12.0...

The fluid and granular consistency of MTA and its elevated setting time make its clinical use difficult. Additives are used to increase the plasticity of CSCs, and thus facilitate material handling.1212. Bortoluzzi EA, Broon NJ, Bramante CM, Garcia RB, Moraes IG, Bernardineli N. Sealing ability of MTA and radiopaque Portland cement with or without calcium chloride for root-end filling. J Endod. 2006;32(9):897-900. doi:10.1016/j.joen.2006.04.006
https://doi.org/10.1016/j.joen.2006.04.0...
Different formulations of this cement, modified with additives and resins, have been proposed to improve the manipulation and consistency of the cement, and have ultimately given rise to modified calcium silicate cements (CSCMs) and resin calcium silicate cements (CSCRs). The addition of 2% and 5% calcium chloride to Portland cement has promoted better setting times, and a biocompatibility similar to that of MTA.1313. Bramante CM, Kato MM, Assis GF, Duarte MA, Bernardineli N, Moraes IG, et al. Biocompatibility and setting time of CPM-MTA and white Portland cement clinker with or without calcium sulfate. J Appl Oral Sci. 2013;21(1):32-6. doi:10.1590/1678-7757201302200
https://doi.org/10.1590/1678-77572013022...
A newly proposal material called calcium silicate-gelatin cement has presented a better setting time, work time and flow than MTA ProRoot. This material has also provided suitable results in regard to proliferation and differentiation of dental pulp cells.1414. Wang CW, Chiang TY, Chang HC, Ding SJ. Physicochemical properties and osteogenic activity of radiopaque calcium silicate-gelatin cements. J Mater Sci Mater Med. 2014;25(9):2193-203. doi:10.1007/s10856-014-5258-5
https://doi.org/10.1007/s10856-014-5258-...

Bosso-Martelo et al.1515. Bosso-Martelo R, Guerreiro-Tanomaru JM, Viapiana R, Berbert FLC, Duarte MAH, Tanomaru-Filho M. Physicochemical properties of calcium silicate cements associated with microparticulate and nanoparticulate radiopacifiers. Clin Oral Investig. 2016 Jan;20(1):83-90. doi:10.1007/s00784-015-1483-7
https://doi.org/10.1007/s00784-015-1483-...
evaluated the physicochemical properties of calcium silicate cements with additives and resins. Some combinations of silicate-based cements and different radiopacifiers have provided a shorter final setting time, low solubility, alkaline pH and calcium ion release. In a recent study, the addition of fluoride-containing radiopacifier ytterbium trifluoride (YbF3) improved the micromechanical and biological characteristics of modified calcium silicate cements, without modifying osteoclast and osteoblast-like cell integrity.1616. Antonijevic D, Jeschke A, Colovic B, Milovanovic P, Jevremovic D, Kisic D, et al. Addition of fluoride-containing radiopacifier improves micromechanical and biological characteristics of modified calcium silicate cements. J Endod. 2015;41(12):2050-7. doi:10.1016/j.joen.2015.09.008
https://doi.org/10.1016/j.joen.2015.09.0...

The biological properties of new cement formulations must be studied for possible application in dentistry. Reparative materials used in contact with periodontal or pulp tissues should not present cytotoxicity or genotoxicity, thereby favoring the repair process.1717. Borra RC, Lotufo MA, Gagioti SM, Barros FM, Andrade PM. A simple method to measure cell viability in proliferation and cytotoxicity assays. Braz Oral Res. 2009;23(3):255-62. doi:10.1590/S1806-83242009000300006
https://doi.org/10.1590/S1806-8324200900...
,1818. Willershausen B, Marroquín BB, Schäfer D, Schulze R. Cytotoxicity of root canal filling materials to three different human cell lines. J Endod. 2000;26(12):703-7. doi:10.1097/00004770-200012000-00007
https://doi.org/10.1097/00004770-2000120...
Genotoxicity describes the property of a chemical agent that damages the genetic information within a cell, causing mutations. Ribeiro et al.1919. Ribeiro DA, Matsumoto MA, Duarte MA, Marques ME, Salvadori DM. In vitro biocompatibility tests of two commercial types of mineral trioxide aggregate. Braz Oral Res. 2005;19(3):183-7. doi:10.1590/S1806-83242005000300005
https://doi.org/10.1590/S1806-8324200500...
also showed that regular and white mineral trioxide aggregate (MTA) cements presented no cytotoxicity and genotoxicity when mouse lymphoma cells were exposed to them, according to the trypan blue and comet assays, respectively. Similar results with Portland cement have shown that none of these materials were cytotoxic when evaluated alone or in association with radiopacifying agents.2020. Ribeiro DA, Sugui MM, Matsumoto MA, Duarte MA, Marques ME, Salvadori DM. Genotoxicity and cytotoxicity of mineral trioxide aggregate and regular and white Portland cements on Chinese hamster ovary (CHO) cells in vitro. Oral Surg Oral Med Oral Pathol Oral Radiol Endod. 2006;101(2):258-61. doi:10.1016/j.tripleo.2005.02.080
https://doi.org/10.1016/j.tripleo.2005.0...
,2121. Gomes-Cornélio AL, Salles LP, Campos-da-Paz M, Cirelli JA, Guerreiro-Tanomaru JM, Tanomaru-Filho M. Cytotoxicity of Portland cement with different radiopacifying agents: a cell death study. J Endod. 2011;37(2):203-10. doi:10.1016/j.joen.2010.11.017
https://doi.org/10.1016/j.joen.2010.11.0...

The aim of this study was to investigate whether the new formulations of pure and modified calcium silicate-based cements induced some type of damage to human osteosarcoma cells (Saos-2). The MTT and apoptosis assays were performed on cement extracts, and the genotoxicity effects were evaluated by comet assay, to monitor the cytotoxic effects.

Methodology

Cell Culture

Human osteoblast cells (SAOS-2 line ATCC HTB-85) were grown as a monolayer culture in T-75 flasks (Corning, Union City, USA) containing Dulbecco Modified Eagle Medium (DMEM-Sigma/Aldrich, St. Louis, USA) supplemented with 10% fetal bovine serum (FBS), penicillin (100 IU/mL), and streptomycin (100 mg/mL) until confluent. The cells were subcultured twice a week at 37 °C, 95% humidity and 5% CO2. Adherent cells in logarithmic growth phase were detached by a mixture of trypsin/EDTA (0.25%) at 37 °C for 3 minutes.

Preparation of extracts

The study procedure followed the methodology described by Gomes-Cornélio et al.2121. Gomes-Cornélio AL, Salles LP, Campos-da-Paz M, Cirelli JA, Guerreiro-Tanomaru JM, Tanomaru-Filho M. Cytotoxicity of Portland cement with different radiopacifying agents: a cell death study. J Endod. 2011;37(2):203-10. doi:10.1016/j.joen.2010.11.017
https://doi.org/10.1016/j.joen.2010.11.0...
One gram of each experimental cement was weighed and manipulated with distilled water, in the recommended proportions, on sterile glass plates (Table). After manipulation, the materials were weighed (1 g) again, and placed in 50 mL Falcon tube lids. All the materials were duly identified, imbibed with damp sterile gauze and taken to the laminar flow chamber, where they remained for 30 minutes under UV light to prevent contamination. After this period, the Falcon tubes were filled with 10 mL of DMEM culture medium containing 10% FBS, the cement-filled lids were fitted onto each tube, which was inverted, so that the materials would come into contact with the culture medium; the tubes were then placed in an oven at 37 °C, 95% humidity and 5% CO2, for 3 hours. Three eluates were selected, as recommended by a previous study,2121. Gomes-Cornélio AL, Salles LP, Campos-da-Paz M, Cirelli JA, Guerreiro-Tanomaru JM, Tanomaru-Filho M. Cytotoxicity of Portland cement with different radiopacifying agents: a cell death study. J Endod. 2011;37(2):203-10. doi:10.1016/j.joen.2010.11.017
https://doi.org/10.1016/j.joen.2010.11.0...
and prepared after contact of the materials with the culture medium: 50 mg/mL, 10 mg/mL and 2 mg/mL before cell exposure.

Table
Experimental materials, source and proportions used.

MTT assay

This assay consists of determining how well the mitochondrial dehydrogenase enzyme converts the water-soluble yellow salt [3-(4,5-dimethyl-thiazoyl)-2,5-diphenyl-tetrazolium bromide - MTT; Sigma/Aldrich] into colored formazan compounds, whose absorbance is proportional to the quantity of live cells. A number of 1 x 105 cells/mL were plated in 24-well culture plates, in triplicate.

After remaining 24 hours in the cell culture with the 3 different eluates of each cement and the controls (C+: 3% hydrogen peroxide, and C-: negative control = cells without treatment), the eluates were aspired and replaced with 900 µl of D-MEM and 5 mg/mL MTT salt, and the plates were incubated for an additional 3 h, in an oven at 37 °C, 95% humidity and 5% CO2. After this period, each well was washed with 1 mL of phosphate buffer (PBS 1X) and aspirated. Then 500 µl of acidified isopropyl alcohol (HCl: isopropyl alcohol, 0.04N) was added to the extract to solubilize the formazan crystals. The samples were transferred to a 96-well plate for readout in triplicate.

The optical density (OD) was measured by an automatic microplate reader (ELx800; BioTek Instruments, Winooski, USA) and submitted to statistical analysis by the variance test (ANOVA), with Bonferroni’s posttest (p < 0.05). Three repetitions of the experiment were performed.

Comet assay

Preparation of Slides

A number of 2 x 106 cells/mL were plated in 24-well culture plates, in triplicate. After 24 hours, the cells were exposed to the 3 different cement eluates and kept in an oven at 37 °C, 95% humidity and 5% CO2, for an additional 24 hours. The experiment was based on the technique described by Sigh et al.2222. Singh NP, McCoy MT, Tice RR, Schneider EL. A simple technique for quantitation of low levels of DNA damage in individual cells. Exp Cell Res. 1998;175(1):184-91. doi:10.1016/0014-4827(88)90265-0
https://doi.org/10.1016/0014-4827(88)902...
After treatment of the cells with the different cement extracts, 200 μl of trypsin/0.25% EDTA (Sigma/Aldrich) was added to each well of the plate for 2 min to detach the cells. After centrifugation (2000 rpm/3 min), each group of cells was resuspended in 200 μl of agarose LMP (low melting point, Sigma/Aldrich) and transferred to slides recently prepared with 1.5% agarose (Sigma/Aldrich). The slides were immersed in lysis solution (NaCl 2.5 M, EDTA 100mM, Tris 10 mM/ 1% Triton X-100, 10% DMSO) and kept at 4 °C overnight. SAOS-2 cells treated with H2O2 (1mM) were used as the positive control.

Electrophoresis

The prepared slides were organized in a horizontal electrophoresis cube, and left in the electrophoresis solution (10 mL 0.2M EDTA + 60 mL 10M NaOH, pH13, to complete 2000 mL milliQ H20) for 20 minutes to allow DNA unwinding. The source was set to 25 V, and the run continued for another 20 minutes. The slides were removed, immersed in a neutralizing solution (0.4M Tris pH7.5) for 15 min, fixed in pure ethanol, and left to dry at room temperature.

Staining and Analysis

An 80 μl volume of ethidium bromide (0.02 mg/mL) was added to stain the slides, and the readouts were immediately taken under a fluorescence microscope (Nikon Corporation, Tokyo, Japan) at 400x magnification. Counts of 100 cells/group were made, and each selected field was photographed. The images were analyzed in the Comet Score software program, and statistically analyzed by the Graphpad Prism 5.03 software program. The counted cells were analyzed, and the same group of materials was compared with both the positive and the negative controls.

The Kruskal-Wallis and Dunn (p < 0.05) tests were performed for the purpose of statistical analysis.

Apoptosis Assay

A number of 1x106 SAOS-2 cells were plated on 24-well culture plates, after remaining in contact with the cement eluates (10 mg/mL). The test was performed with the FITC Annexin V Apoptosis Detection Kit I (BD Biosciences, Pharmingen, San Jose, USA) in a 24-hour period. Afterwards, the cells were washed and collected from the culture plate wells containing nonenzymatic reagent (cell dissociation buffer - Gibco/Carlsbad, California, USA), resuspended in binding buffer 1X (0.1 M Hepes/NaOH; 1.4M NaCl; 25mM CaCl2 – pH: 7.4), and then stained with apoptosis markers: FITC Annexin V and/or PI (propidium iodide staining solution) – 50μg/mL; these same cells also underwent unmarked controls and the positive control (Camptothecin 1mM- Sigma/Aldrich). All the Eppendorf tubes were incubated in a dark environment for 15 min, and 400 μl of 1X binding buffer was added to each sample. Analyses were performed in a Flow Cytometer (BD FACS Verse 4C), in accordance with the parameters of the kit: viable cells (FITC-/ PI-); cells at the stage of initial apoptosis (FITC+/ PI-); cells at the stage of final apoptosis (FITC+/ PI+); cellular necrosis (FITC -/ PI+). The results were submitted to statistical analysis of variance (ANOVA), with Bonferroni’s posttest (p < 0.05). The experiment was conducted in triplicate.

Results

MTT assay

The cements evaluated presented biocompatibility, with results similar to those of the negative control group (p < 0.05), except for CSC 50 mg/mL and CSCR3 10 mg/mL, as shown in Figure 1.

Figure 1
Cell viability of SAOS-2, after being cultivated with eluates of the cements in different concentrations (50mg/mL; 10mg/mL; 2mg/mL) in a period of 24 hours. NC represents the negative control (untreated cells), and PC represents the positive control (3% hydrogen peroxide) for 10 minutes. Different letters represent results that differed statistically among one another, within the same concentration. Analysis of Variance, Bonferroni (p<0.05).

Comet Assay

All of the CSCs evaluated, with the exception of the pure CSC, presented genotoxicity in the concentration of 50 mg/mL, compared with the control, whereas CSC and CSCR2 presented no genotoxicity in the concentration of 10 mg/mL, compared with the negative control. In the last concentration of 2 mg/mL, all the cements, except for CSCM, were similar to those of the negative control group (p < 0.05), (Figure 2).

Figure 2
Genotoxicity represented by % of DNA in the tail, in the SAOS-2 cell lineage treated with eluates of 50, 10 and 2 mg/mL for 24 hours. C-: Negative control (untreated cells), C+: Positive control (1mM of hydrogen peroxide for 10 min). Results are expressed as a % of DNA in the tail of 100 cells per concentration and controls, and analyzed by Kruskal-Wallis, with the Dunn posttest (treated vs. C-).

Apoptosis Assay

Histograms were used to represent the percentage of viable osteoblast cells (SAOS-2), and analyze the initial and final stage of apoptosis and necrosis, within a 24-hour period. In regard to cell viability, groups CSCR1 and CSCR2 were found to be similar to the negative control (cells without treatment), unlike CSCR3, which displayed low cell viability (p < 0.05). Groups CSC and CSCM presented slightly higher viability values than those of the negative control. In the initial stage of apoptosis, all the groups were found to be different from the negative control, with higher percentages, and the CSCR3 group showed a higher rate of initial apoptosis (p < 0.05). The experimental groups showed lower values of late apoptosis and necrosis, compared with the negative control (p < 0.05), (Figure 3).

Figure 3
(A) Flow cytometry analysis of SAOS-2 viability, mortality by apoptosis or necrosis after exposure to different calcium silicate-based cements on the concentration of 10mg/mL after 24 hours. Cells exposed to medium were the negative control and cells treated with hydrogen peroxide (1 mM) were the positive control group. (B) Representative 2-dimensional flow cytometry dot plot of data derived from FITC-AnV and PE incorporated PI stained SAOS-2 cells of control, CSC, CSCM, CSCR1, CSCR2 and CSCR3 groups. Bars with different letters represent significant differences between groups in each population analyzed. The population of living cells (LC) (annexin-/ PI-), initial apoptosis (IA) (annexin+/ PI-), late apoptosisor secondary necrosis (LA) (annexin+/ PI+), and necrotic (N) (annexin-/ PI+)cells are represented in the left inferior, right inferior, right superior and left superior quadrants, respectively. PC = positive control, NC = negative control.

Discussion

Additives have been incorporated into Portland cement to improve its physical and chemical properties. New calcium silicate-based cements have also been studied,2323. Camilleri J. The biocompatibility of modified experimental Portland cements with potential for use in dentistry. Int Endod J. 2008;41(12):1107-14. doi:10.1111/j.1365-2591.2008.01483.x
https://doi.org/10.1111/j.1365-2591.2008...
,2424. Amoroso-Silva PA, Marciano MA, Guimarães BM, Duarte MAH, Sanson AF, Moraes IG. Apical adaptation, sealing ability and push-out bond strength of five root-end filling materials. Braz Oral Res [Internet]. 2014 Aug 26 [cited 2016 Feb 17];28(1):1-6. Available from: http://www.scielo.br/scielo.php?script=sci_arttext&pid=S1806-83242014000100252&lng=en&nrm=iso&tlng=en. doi:10.1590/1807-3107BOR-2014.vol28.0043
http://www.scielo.br/scielo.php?script=s...
and some of the modified calcium silicate and resin cements under study may present the potential for clinical use. CSCM is a modified calcium silicate cement that contains mineral aggregates, additives and pigments. Resin calcium silicate cements (CSCRs) not only have mineral aggregates, additives and pigments, but also resin components in their composition, aimed at improving their manipulation and setting time. However, the addition of composites in cements may interfere and harm their biological properties and bioactivity.1313. Bramante CM, Kato MM, Assis GF, Duarte MA, Bernardineli N, Moraes IG, et al. Biocompatibility and setting time of CPM-MTA and white Portland cement clinker with or without calcium sulfate. J Appl Oral Sci. 2013;21(1):32-6. doi:10.1590/1678-7757201302200
https://doi.org/10.1590/1678-77572013022...

The immortalized osteoblast cell lineage was used in this study, because of its reproducibility capabilities, and because its relationship with the bone repair process in tissues2525. Mansur AA, Mansur HS. Preparation and characterization of 3D porous ceramic scaffolds based on portland cement for bone tissue engineering. J Mater Sci Mater Med. 2009 Feb;20(2):497-505. doi:10.1007/s10856-008-3612-1
https://doi.org/10.1007/s10856-008-3612-...
,2626. Salles LP, Gomes-Cornélio AL, Guimarães FC, Herrera BS, Bao SN, Rossa-Junior C, et al. Mineral trioxide aggregate- based endodontic sealer stimulates hydroxyapatite nucleation in human osteoblast-like cell culture. J Endod. 2012;38(7):971-6. doi:10.1016/j.joen.2012.02.018
https://doi.org/10.1016/j.joen.2012.02.0...
makes it ideal for vitro assays researching new endodontic and retrofilling materials. Modareszadeh et al.2727. Modareszadeh MR, Di Fiore PM, Tipton DA, Salamat N. Cytotoxicity and alkaline phosphatase activity evaluation of endosequence root repair material. J Endod. 2012;38(8):1101-5. doi:10.1016/j.joen.2012.04.014
https://doi.org/10.1016/j.joen.2012.04.0...
evaluated the cytotoxicity and bioactivity of the Endo sequence bioceramic material (Brasseler, Savannah, USA) in human osteoblast cells (SAOS-2), and reported the importance of these cells in the mineralization and repair process. Gandolfi et al.2828. Gandolfi MG, Shah SN, Feng R, Prati C, Akintoye SO. Biomimetic calcium-silicate cements support differentiation of human orofacial mesenchymal stem cells. J Endod. 2011;37(8):1102-8. doi:10.1016/j.joen.2011.05.009
https://doi.org/10.1016/j.joen.2011.05.0...
confirmed that calcium silicate-based cements and MTA are good substrates for osteoblast growth, and induce cell proliferation, even when fresh cements are used, as was done in the present study.

The results of the present study showed that calcium silicate-based cements did not present cytotoxicity, compared with the positive control (3% hydrogen peroxide), and were similar to the negative control (untreated cells) particularly in the concentrations of 10 mg/mL and 2 mg/mL. Favorable results have been observed for pure and/or modified calcium silicate-based cements, either associated with radiopacifying agents, or not.2121. Gomes-Cornélio AL, Salles LP, Campos-da-Paz M, Cirelli JA, Guerreiro-Tanomaru JM, Tanomaru-Filho M. Cytotoxicity of Portland cement with different radiopacifying agents: a cell death study. J Endod. 2011;37(2):203-10. doi:10.1016/j.joen.2010.11.017
https://doi.org/10.1016/j.joen.2010.11.0...
,2929. Lee SJ, Chung J, Na HS, Park EJ, Jeon HJ, Kim HC. Characteristics of novel root-end filling material using epoxy resin and Portland cement. Clin Oral Investig. 2013;17(3):1009-15. doi:10.1007/s00784-012-0782-5
https://doi.org/10.1007/s00784-012-0782-...
A newly developed CSC, with zirconium oxide (ZrO2), named Ortho-MTA (OMTA; BioMTA, Seoul, Korea) has promoted an inflammatory response and odontoblastic differentiation similar to Biodentine and MTA Angelus in human dental pulp cells (hDPCs).3030. Chang SW, Lee SY, Ann HJ, Kum KY, Kim EC. effects of calcium silicate endodontic cements on biocompatibility and mineralization-inducing potentials in human dental pulp cells. J Endod. 2014;40(8):1194-200. doi:10.1016/j.joen.2014.01.001
https://doi.org/10.1016/j.joen.2014.01.0...
Furthermore, CSC has been found to stimulate osteogenesis in a co-culture of macrophage cells (Raw 264.7) and osteoblast cells (MC3T3-E1), with improved proliferation and higher calcium deposition than cells in a monoculture.3131. Tu MG, Chen YW, Shie MY. Macrophage-mediated osteogenesis activation in co-culture with osteoblast on calcium silicate cement. J Mater Sci Mater Med. 2015;26(12):276. doi:10.1007/s10856-015-5607-z
https://doi.org/10.1007/s10856-015-5607-...
In our recent study, the silicate-based cement associated with ZrO2 exhibited a viability rate similar to that of MTA Plus and Biodentine in osteoblast-like cells.3232. Gomes-Cornélio AL, Rodrigues EM, Salles LP, Mestieri LB, Faria G, Guerreiro-Tanomaru JM, et al. Bioactivity of MTA Plus, Biodentine and experimental calcium silicate-based cements in human osteoblast-like cells. Int Endod J. 2015 Nov 26 [cited 2016 Feb 17]. Available from: http://onlinelibrary.wiley.com/doi/10.1111/iej.12589/abstract;jsessionid=A10B9DC41710A274DA102DCE9FEB2674.f02t04?systemMessage=Wiley+Online+Library+will+be+unavailable+on+Saturday+27th+February+from+09%3A00-14%3A00+GMT+%2F+04%3A00-09%3A00+EST+%2F+17%3A00-22%3A00+SGT+for+essential+maintenance.++Apologies+for+the+inconvenience. doi:10.1111/iej.12589.
http://onlinelibrary.wiley.com/doi/10.11...
However, the MTT assay could show a false-positive result,3333. Berridge MV, Tan AS. Characterization of the cellular reduction of 3-(4,5-dimethylthiazol-2-yl)-2,5-diphenyltetrazolium bromide (MTT): subcellular localization, substrate dependence, and involvement of mitochondrial electron transport in MTT reduction. Arch Biochem Biophys. 1993;303(2):474-82. doi:10.1006/abbi.1993.1311
https://doi.org/10.1006/abbi.1993.1311...
thus making it important to perform other cytotoxicity tests.

Some studies have shown that MTA does not induce significant apoptosis and/or necrosis in distinct cell lineages.3333. Berridge MV, Tan AS. Characterization of the cellular reduction of 3-(4,5-dimethylthiazol-2-yl)-2,5-diphenyltetrazolium bromide (MTT): subcellular localization, substrate dependence, and involvement of mitochondrial electron transport in MTT reduction. Arch Biochem Biophys. 1993;303(2):474-82. doi:10.1006/abbi.1993.1311
https://doi.org/10.1006/abbi.1993.1311...
,3434. Moghaddame-Jafari S, Mantellini MG, Botero TM, McDonald NJ, Nör JE. Effect of ProRoot MTA on pulp cell apoptosis and proliferation in vitro. J Endod. 2005;31(5):387-91. doi:10.1097/01.don.0000145423.89539.d7
https://doi.org/10.1097/01.don.000014542...
The flow cytometry experiment using the FITC Annexin V Apoptosis Detection Kit I (BD Biosciences) was used to analyze the following: intact cells; cells in initial apoptosis, where FITC binds to phosphatidylserine (a component of the cell membrane), which is found inverted in the cells at this stage; and cells in final apoptosis and necrosis. In this final stage, in addition to the positive binding of FITC, there is also the binding of PI (propidium iodide) to the genetic material of the cell, since the membrane is completely damaged at this stage of cell death, thus allowing entry of the marker. Gorduysus et al.3535. Gorduysus M, Avcu N, Gorduysus O, Pekel A, Baran Y, Avcu F, et al. Cytotoxic effects of four different endodontic materials in human periodontal ligament fibroblasts. J Endod. 2007;33(12):1450-4. doi:10.1016/j.joen.2007.08.017
https://doi.org/10.1016/j.joen.2007.08.0...
used the same methodology to evaluate the type of cell death of human fibroblasts in different endodontic materials. MTA behaved in a manner very similar to that of the control, with high percentages of viable cells; however, the materials tested [Diaket (ESPE, Seefeld, Germany) Endion (VOCO, Cuxhaven, Germany) and CYMED 8410 (NANO, Kaohsiung, Taiwan)] induced high percentages of apoptosis and necrosis, in comparison with the control.

CSCR1 and CSCR2 were similar to the control as regards cell viability, unlike CSCR3, which had a lower percentage of cell viability (p < 0.05). Groups CSC and CSCM presented higher viability values than those of the negative control (p < 0.05). All the experimental groups induced initial apoptosis, but not late apoptosis or necrosis, compared with the control (p < 0.05). It is known that endoplasmic reticulum stress caused by an excess of Ca+2 ions may lead to apoptosis;3636. Franco R, Cidlowski JA. Apoptosis and glutathione: beyond an antioxidant. Cell Death Differ. 2009;16(10):1303-14. doi:10.1038/cdd.2009.107
https://doi.org/10.1038/cdd.2009.107...
this could be one of the explanations for why the groups treated with different calcium silicate-based cements had a rapid onset of apoptosis. Eid et al.3737. Eid AA, Gosier JL, Primus CM, Hammond BD, Susin LF, Pashley DH, et al. In vitro biocompatibility and oxidative stress profiles of different hydraulic calcium silicate cements. J Endod. 2014;40(2):255-60. doi:10.1016/j.joen.2013.07.009
https://doi.org/10.1016/j.joen.2013.07.0...
also found a higher percentage of apoptosis in cells exposed to the calcium silicate-based MTA Plus and MTA Angelus materials, suggesting that the initial sites of irreversible damage by cytotoxic agents are extracellular, while the nuclear membranes of these cells still remain intact.

The comet assay suggested damage to DNA, chromosome breakage, altered DNA repair and cellular transformation.2020. Ribeiro DA, Sugui MM, Matsumoto MA, Duarte MA, Marques ME, Salvadori DM. Genotoxicity and cytotoxicity of mineral trioxide aggregate and regular and white Portland cements on Chinese hamster ovary (CHO) cells in vitro. Oral Surg Oral Med Oral Pathol Oral Radiol Endod. 2006;101(2):258-61. doi:10.1016/j.tripleo.2005.02.080
https://doi.org/10.1016/j.tripleo.2005.0...
Among the various parameters calculated by this method, one of the most widely used indicators of DNA damage is the length of the comet tail, which is a virtual measurement calculated by the computed image analysis system, considering both the duration of DNA migration in the comet tail and the intensity of the tail.3838. Tice RR, Agurell E, Anderson D, Burlinson B, Hartmann A, Kobayashi H, et al. Single cell gel/comet assay: guidelines for in vitro and in vivo genetic toxicology testing. Environ Mol Mutagen. 2000;35(3):206-21. doi:10.1002/(SICI)1098-2280(2000)35:3<206::AID-EM8>3.0.CO;2-J

The results of this study revealed that CSC and CSCR2 performed outstandingly in the concentration of 10 mg/mL, since they presented no genotoxicity compared with the negative control. These results for pure CSC corroborate those of other studies that have demonstrated its biocompatibility.1919. Ribeiro DA, Matsumoto MA, Duarte MA, Marques ME, Salvadori DM. In vitro biocompatibility tests of two commercial types of mineral trioxide aggregate. Braz Oral Res. 2005;19(3):183-7. doi:10.1590/S1806-83242005000300005
https://doi.org/10.1590/S1806-8324200500...
,2020. Ribeiro DA, Sugui MM, Matsumoto MA, Duarte MA, Marques ME, Salvadori DM. Genotoxicity and cytotoxicity of mineral trioxide aggregate and regular and white Portland cements on Chinese hamster ovary (CHO) cells in vitro. Oral Surg Oral Med Oral Pathol Oral Radiol Endod. 2006;101(2):258-61. doi:10.1016/j.tripleo.2005.02.080
https://doi.org/10.1016/j.tripleo.2005.0...
,2121. Gomes-Cornélio AL, Salles LP, Campos-da-Paz M, Cirelli JA, Guerreiro-Tanomaru JM, Tanomaru-Filho M. Cytotoxicity of Portland cement with different radiopacifying agents: a cell death study. J Endod. 2011;37(2):203-10. doi:10.1016/j.joen.2010.11.017
https://doi.org/10.1016/j.joen.2010.11.0...
The low genotoxic risk associated with a new cement based on dicalcium- and tricalcium-silicate (CS) with hydroxyapatite (HA) was observed using the comet assay and human peripheral blood lymphocytes.3939. Opačić-Galić V, Petrović V, Zivković S, Jokanović V, Nikolić B, Knežević-Vukčević J, et al. New nanostructural biomaterials based on actives silicate systems and hydroxyapatite: characterization and genotoxicity in human peripheral blood lymphocytes. Int Endod J. 2013;46(6):506-16. doi:10.1111/iej.12017
https://doi.org/10.1111/iej.12017...
Biosilicate® analysis of genotoxicity showed no DNA damage in lineages, osteoblasts or fibroblasts, in all the evaluation periods (24, 72, and 96 hours).4040. Kido HW, Oliveira P, Parizotto NA, Crovace MC, Zanotto ED, Peitl-Filho O, et al. Histopathological, cytotoxicity and genotoxicity evaluation of Biosilicate® glass-ceramic scaffolds. J Biomed Mater Res A. 2013;101(3):667-73. doi:10.1002/jbm.a.34360
https://doi.org/10.1002/jbm.a.34360...

The different modified CSCs presented appropriate cell viability results. A high number of living cells were preserved in the cells exposed to CSCs, although the percentage of apoptosis increased slightly. Genotoxicity analysis indicated that the CSCs did not induce DNA damage in osteoblast-like cells (Saos-2) at the highest CSC dilution. These results suggest that CSCs have a good potential for use as a reparative material. However, additional studies are needed to research new CSCs.

Acknowledgements

This study received financial support from the Fundação de Amparo à Pesquisa do Estado de São Paulo - FAPESP, process no. 2011/13116-1, 2011/18239-4 and 2012/13268-9.

References

  • 1
    Torabinejad M, Watson TF, Pitt Ford TR. Sealing ability of a mineral trioxide aggregate when used as a root end filling material. J Endod. 1993;19(12):591-5. doi:10.1016/S0099-2399(06)80271-2
    » https://doi.org/10.1016/S0099-2399(06)80271-2
  • 2
    Torabinejad M, Parirokh M. Mineral trioxide aggregate: a comprehensive literature review - part II: leakage and biocompatibility investigations. J Endod. 2010 Feb;36(2):190-202. doi:10.1016/j.joen.2009.09.010
    » https://doi.org/10.1016/j.joen.2009.09.010
  • 3
    Tanomaru-Filho M, Bosso R, Viapiana R, Guerreiro-Tanomaru JM. Radiopacity and flow of different endodontic sealers. Acta Odontol Latinoam. 2013;26(2):121-5.
  • 4
    Pelliccioni GA, Ciapetti G, Cenni E, Granchi D, Nanni M, Pagani S, et al. Evaluation of osteoblast-like cell response to Proroot MTA (mineral trioxide aggregate) cement. J Mater Sci Mater Med. 2004;15(2):167-73. doi:10.1023/B:JMSM.0000011819.26935.47
    » https://doi.org/10.1023/B:JMSM.0000011819.26935.47
  • 5
    Bogen G, Kim JS, Bakland LK. Direct pulp capping with mineral trioxide aggregate: an observational study. J Am Dent Assoc. 2008;139(3):305-15; quiz 305-15. Erratum in: J Am Dent Assoc. 2008;139(5):541.
  • 6
    Oliveira MG, Xavier CB, Demarco FF, Pinheiro AL, Costa AT, Pozza DH. Comparative chemical study of MTA and Portland cements. Braz Dent J. 2007;18(1):3-7. doi:10.1590/S0103-64402007000100002
    » https://doi.org/10.1590/S0103-64402007000100002
  • 7
    Gonçalves JL, Viapiana R, Miranda CE, Borges AH, Cruz Filho AM. Evaluation of physico-chemical properties of Portland cements and MTA. Braz Oral Res. 2010;24(3):277-83. doi:10.1590/S1806-83242010000300004
    » https://doi.org/10.1590/S1806-83242010000300004
  • 8
    Maeno S, Niki Y, Matsumoto H, Morioka H, Yatabe T, Funayama A, et al. The effect of calcium ion concentration on osteoblast viability, proliferation and differentiation in monolayer and 3D culture. Biomaterials. 2005;26(23):4847-55. doi:10.1016/j.biomaterials.2005.01.006
    » https://doi.org/10.1016/j.biomaterials.2005.01.006
  • 9
    Sun J, Wei L, Liu X, Li J, Li B, Wang G, et al. Influences of ionic dissolution products of dicalcium silicate coating on osteoblastic proliferation, differentiation and gene expression. Acta Biomater. 2009;5(4):1284-93. doi:10.1016/j.actbio.2008.10.011
    » https://doi.org/10.1016/j.actbio.2008.10.011
  • 10
    Eid AA, Niu L-n, Primus CM, Opperman LA, Watanabe I, Pashley DH, et al. In vitro osteogenic/dentinogenic potential of an experimental calcium aluminosilicate cement. J Endod. 2013;39(9):1161-6. doi:10.1016/j.joen.2013.04.005
    » https://doi.org/10.1016/j.joen.2013.04.005
  • 11
    Chen CL, Kao CT, Ding SJ, Shie MY, Huang TH. Expression of the inflammatory marker cyclooxygenase-2 in dental pulp cells cultured with mineral trioxide aggregate or calcium silicate cements. J Endod. 2010;36(3):465-8. doi:10.1016/j.joen.2009.12.008
    » https://doi.org/10.1016/j.joen.2009.12.008
  • 12
    Bortoluzzi EA, Broon NJ, Bramante CM, Garcia RB, Moraes IG, Bernardineli N. Sealing ability of MTA and radiopaque Portland cement with or without calcium chloride for root-end filling. J Endod. 2006;32(9):897-900. doi:10.1016/j.joen.2006.04.006
    » https://doi.org/10.1016/j.joen.2006.04.006
  • 13
    Bramante CM, Kato MM, Assis GF, Duarte MA, Bernardineli N, Moraes IG, et al. Biocompatibility and setting time of CPM-MTA and white Portland cement clinker with or without calcium sulfate. J Appl Oral Sci. 2013;21(1):32-6. doi:10.1590/1678-7757201302200
    » https://doi.org/10.1590/1678-7757201302200
  • 14
    Wang CW, Chiang TY, Chang HC, Ding SJ. Physicochemical properties and osteogenic activity of radiopaque calcium silicate-gelatin cements. J Mater Sci Mater Med. 2014;25(9):2193-203. doi:10.1007/s10856-014-5258-5
    » https://doi.org/10.1007/s10856-014-5258-5
  • 15
    Bosso-Martelo R, Guerreiro-Tanomaru JM, Viapiana R, Berbert FLC, Duarte MAH, Tanomaru-Filho M. Physicochemical properties of calcium silicate cements associated with microparticulate and nanoparticulate radiopacifiers. Clin Oral Investig. 2016 Jan;20(1):83-90. doi:10.1007/s00784-015-1483-7
    » https://doi.org/10.1007/s00784-015-1483-7
  • 16
    Antonijevic D, Jeschke A, Colovic B, Milovanovic P, Jevremovic D, Kisic D, et al. Addition of fluoride-containing radiopacifier improves micromechanical and biological characteristics of modified calcium silicate cements. J Endod. 2015;41(12):2050-7. doi:10.1016/j.joen.2015.09.008
    » https://doi.org/10.1016/j.joen.2015.09.008
  • 17
    Borra RC, Lotufo MA, Gagioti SM, Barros FM, Andrade PM. A simple method to measure cell viability in proliferation and cytotoxicity assays. Braz Oral Res. 2009;23(3):255-62. doi:10.1590/S1806-83242009000300006
    » https://doi.org/10.1590/S1806-83242009000300006
  • 18
    Willershausen B, Marroquín BB, Schäfer D, Schulze R. Cytotoxicity of root canal filling materials to three different human cell lines. J Endod. 2000;26(12):703-7. doi:10.1097/00004770-200012000-00007
    » https://doi.org/10.1097/00004770-200012000-00007
  • 19
    Ribeiro DA, Matsumoto MA, Duarte MA, Marques ME, Salvadori DM. In vitro biocompatibility tests of two commercial types of mineral trioxide aggregate. Braz Oral Res. 2005;19(3):183-7. doi:10.1590/S1806-83242005000300005
    » https://doi.org/10.1590/S1806-83242005000300005
  • 20
    Ribeiro DA, Sugui MM, Matsumoto MA, Duarte MA, Marques ME, Salvadori DM. Genotoxicity and cytotoxicity of mineral trioxide aggregate and regular and white Portland cements on Chinese hamster ovary (CHO) cells in vitro. Oral Surg Oral Med Oral Pathol Oral Radiol Endod. 2006;101(2):258-61. doi:10.1016/j.tripleo.2005.02.080
    » https://doi.org/10.1016/j.tripleo.2005.02.080
  • 21
    Gomes-Cornélio AL, Salles LP, Campos-da-Paz M, Cirelli JA, Guerreiro-Tanomaru JM, Tanomaru-Filho M. Cytotoxicity of Portland cement with different radiopacifying agents: a cell death study. J Endod. 2011;37(2):203-10. doi:10.1016/j.joen.2010.11.017
    » https://doi.org/10.1016/j.joen.2010.11.017
  • 22
    Singh NP, McCoy MT, Tice RR, Schneider EL. A simple technique for quantitation of low levels of DNA damage in individual cells. Exp Cell Res. 1998;175(1):184-91. doi:10.1016/0014-4827(88)90265-0
    » https://doi.org/10.1016/0014-4827(88)90265-0
  • 23
    Camilleri J. The biocompatibility of modified experimental Portland cements with potential for use in dentistry. Int Endod J. 2008;41(12):1107-14. doi:10.1111/j.1365-2591.2008.01483.x
    » https://doi.org/10.1111/j.1365-2591.2008.01483.x
  • 24
    Amoroso-Silva PA, Marciano MA, Guimarães BM, Duarte MAH, Sanson AF, Moraes IG. Apical adaptation, sealing ability and push-out bond strength of five root-end filling materials. Braz Oral Res [Internet]. 2014 Aug 26 [cited 2016 Feb 17];28(1):1-6. Available from: http://www.scielo.br/scielo.php?script=sci_arttext&pid=S1806-83242014000100252&lng=en&nrm=iso&tlng=en doi:10.1590/1807-3107BOR-2014.vol28.0043
    » https://doi.org/10.1590/1807-3107BOR-2014.vol28.0043» http://www.scielo.br/scielo.php?script=sci_arttext&pid=S1806-83242014000100252&lng=en&nrm=iso&tlng=en
  • 25
    Mansur AA, Mansur HS. Preparation and characterization of 3D porous ceramic scaffolds based on portland cement for bone tissue engineering. J Mater Sci Mater Med. 2009 Feb;20(2):497-505. doi:10.1007/s10856-008-3612-1
    » https://doi.org/10.1007/s10856-008-3612-1
  • 26
    Salles LP, Gomes-Cornélio AL, Guimarães FC, Herrera BS, Bao SN, Rossa-Junior C, et al. Mineral trioxide aggregate- based endodontic sealer stimulates hydroxyapatite nucleation in human osteoblast-like cell culture. J Endod. 2012;38(7):971-6. doi:10.1016/j.joen.2012.02.018
    » https://doi.org/10.1016/j.joen.2012.02.018
  • 27
    Modareszadeh MR, Di Fiore PM, Tipton DA, Salamat N. Cytotoxicity and alkaline phosphatase activity evaluation of endosequence root repair material. J Endod. 2012;38(8):1101-5. doi:10.1016/j.joen.2012.04.014
    » https://doi.org/10.1016/j.joen.2012.04.014
  • 28
    Gandolfi MG, Shah SN, Feng R, Prati C, Akintoye SO. Biomimetic calcium-silicate cements support differentiation of human orofacial mesenchymal stem cells. J Endod. 2011;37(8):1102-8. doi:10.1016/j.joen.2011.05.009
    » https://doi.org/10.1016/j.joen.2011.05.009
  • 29
    Lee SJ, Chung J, Na HS, Park EJ, Jeon HJ, Kim HC. Characteristics of novel root-end filling material using epoxy resin and Portland cement. Clin Oral Investig. 2013;17(3):1009-15. doi:10.1007/s00784-012-0782-5
    » https://doi.org/10.1007/s00784-012-0782-5
  • 30
    Chang SW, Lee SY, Ann HJ, Kum KY, Kim EC. effects of calcium silicate endodontic cements on biocompatibility and mineralization-inducing potentials in human dental pulp cells. J Endod. 2014;40(8):1194-200. doi:10.1016/j.joen.2014.01.001
    » https://doi.org/10.1016/j.joen.2014.01.001
  • 31
    Tu MG, Chen YW, Shie MY. Macrophage-mediated osteogenesis activation in co-culture with osteoblast on calcium silicate cement. J Mater Sci Mater Med. 2015;26(12):276. doi:10.1007/s10856-015-5607-z
    » https://doi.org/10.1007/s10856-015-5607-z
  • 32
    Gomes-Cornélio AL, Rodrigues EM, Salles LP, Mestieri LB, Faria G, Guerreiro-Tanomaru JM, et al. Bioactivity of MTA Plus, Biodentine and experimental calcium silicate-based cements in human osteoblast-like cells. Int Endod J. 2015 Nov 26 [cited 2016 Feb 17]. Available from: http://onlinelibrary.wiley.com/doi/10.1111/iej.12589/abstract;jsessionid=A10B9DC41710A274DA102DCE9FEB2674.f02t04?systemMessage=Wiley+Online+Library+will+be+unavailable+on+Saturday+27th+February+from+09%3A00-14%3A00+GMT+%2F+04%3A00-09%3A00+EST+%2F+17%3A00-22%3A00+SGT+for+essential+maintenance.++Apologies+for+the+inconvenience doi:10.1111/iej.12589.
    » https://doi.org/10.1111/iej.12589.» http://onlinelibrary.wiley.com/doi/10.1111/iej.12589/abstract;jsessionid=A10B9DC41710A274DA102DCE9FEB2674.f02t04?systemMessage=Wiley+Online+Library+will+be+unavailable+on+Saturday+27th+February+from+09%3A00-14%3A00+GMT+%2F+04%3A00-09%3A00+EST+%2F+17%3A00-22%3A00+SGT+for+essential+maintenance.++Apologies+for+the+inconvenience
  • 33
    Berridge MV, Tan AS. Characterization of the cellular reduction of 3-(4,5-dimethylthiazol-2-yl)-2,5-diphenyltetrazolium bromide (MTT): subcellular localization, substrate dependence, and involvement of mitochondrial electron transport in MTT reduction. Arch Biochem Biophys. 1993;303(2):474-82. doi:10.1006/abbi.1993.1311
    » https://doi.org/10.1006/abbi.1993.1311
  • 34
    Moghaddame-Jafari S, Mantellini MG, Botero TM, McDonald NJ, Nör JE. Effect of ProRoot MTA on pulp cell apoptosis and proliferation in vitro. J Endod. 2005;31(5):387-91. doi:10.1097/01.don.0000145423.89539.d7
    » https://doi.org/10.1097/01.don.0000145423.89539.d7
  • 35
    Gorduysus M, Avcu N, Gorduysus O, Pekel A, Baran Y, Avcu F, et al. Cytotoxic effects of four different endodontic materials in human periodontal ligament fibroblasts. J Endod. 2007;33(12):1450-4. doi:10.1016/j.joen.2007.08.017
    » https://doi.org/10.1016/j.joen.2007.08.017
  • 36
    Franco R, Cidlowski JA. Apoptosis and glutathione: beyond an antioxidant. Cell Death Differ. 2009;16(10):1303-14. doi:10.1038/cdd.2009.107
    » https://doi.org/10.1038/cdd.2009.107
  • 37
    Eid AA, Gosier JL, Primus CM, Hammond BD, Susin LF, Pashley DH, et al. In vitro biocompatibility and oxidative stress profiles of different hydraulic calcium silicate cements. J Endod. 2014;40(2):255-60. doi:10.1016/j.joen.2013.07.009
    » https://doi.org/10.1016/j.joen.2013.07.009
  • 38
    Tice RR, Agurell E, Anderson D, Burlinson B, Hartmann A, Kobayashi H, et al. Single cell gel/comet assay: guidelines for in vitro and in vivo genetic toxicology testing. Environ Mol Mutagen. 2000;35(3):206-21. doi:10.1002/(SICI)1098-2280(2000)35:3<206::AID-EM8>3.0.CO;2-J
  • 39
    Opačić-Galić V, Petrović V, Zivković S, Jokanović V, Nikolić B, Knežević-Vukčević J, et al. New nanostructural biomaterials based on actives silicate systems and hydroxyapatite: characterization and genotoxicity in human peripheral blood lymphocytes. Int Endod J. 2013;46(6):506-16. doi:10.1111/iej.12017
    » https://doi.org/10.1111/iej.12017
  • 40
    Kido HW, Oliveira P, Parizotto NA, Crovace MC, Zanotto ED, Peitl-Filho O, et al. Histopathological, cytotoxicity and genotoxicity evaluation of Biosilicate® glass-ceramic scaffolds. J Biomed Mater Res A. 2013;101(3):667-73. doi:10.1002/jbm.a.34360
    » https://doi.org/10.1002/jbm.a.34360

Publication Dates

  • Publication in this collection
    2016

History

  • Received
    23 Sept 2015
  • Accepted
    27 Jan 2016
  • Reviewed
    17 Feb 2016
Sociedade Brasileira de Pesquisa Odontológica - SBPqO Av. Prof. Lineu Prestes, 2227, 05508-000 São Paulo SP - Brazil, Tel. (55 11) 3044-2393/(55 11) 9-7557-1244 - São Paulo - SP - Brazil