Open-access Effect of Heat Treatment on Microstructures and Mechanical Properties of 6061 Aluminum Alloy Fabricated by Rotational Deposition Additive Manufacturing (RDAM)

Abstract

This work systematically investigates the effect of a 480 °C/2 h solution + 120 °C/3 h + 155 °C/6 h ageing on the microstructure and mechanical performance of 6061-T5 aluminium alloy produced by rotational deposition-based additive manufacturing (RDAM). The treatment promotes the precipitation of β″ strengthening phases within the α-Al matrix, refines the grain structure and eliminates the inter-layer processing traces characteristic of the as-deposited condition. The hardness of alloys increases by 5~6%, reaching a maximum average value of 57.3 HV on the top surface after duplex ageing. Tensile properties indicated that along the deposition X-axis direction, the duplex-aged specimens attain an ultimate tensile strength (UTS) of 385 MPa, which is an 82% improvement over the 211.6 MPa recorded in the as-deposited state. In the build Z-axis direction, the UTS rise to 222.3 MPa, corresponding to a 72% increase. The lower increment in the Z-axis direction is attributed to residual micro-voids at inter-layer interfaces and heterogeneous precipitate distributions that localize plastic deformation. In addition, the top surface of the aged alloy exhibits a free-corrosion potential of -0.506 V, while the side surface of alloy displays a corrosion-current density of 4.58×10−8 A·cm−2, representing a substantial improvement over the as-deposited condition. Consequently, the optimised duplex-ageing route effectively upgrades the properties of RDAM-produced 6061 aluminium alloy, providing a critical foundation for additive fabricating high-performance aluminium alloys.

Keywords:
Rotational deposition additive manufacturing (RDAM); Aluminium alloy; Heat treatment; Microstructures; Mechanical properties; Corrosion


1. Introduction

6061 aluminum alloy has garnered significant attention in the aerospace and automotive industries owing to its favorable properties, including low density, high elastic modulus, excellent specific strength, superior corrosion resistance, and recyclability1-3. Despite these advantageous characteristics, the limited surface performance of aluminum alloys, particularly their low wear resistance and insufficient microhardness, remains a critical limitation that may hinder broader application4. In general, aluminum alloys exhibit good ductility, low density, and strong corrosion resistance. However, they are inherently susceptible to low hardness and poor wear resistance5-7. To enhance its applicability in various engineering fields, there are currently a variety of heat treatment technologies8. It should be noted that conventional manufacturing methods for aluminum present several challenges, particularly those associated with melting-based processes such as casting, welding, selective laser melting9, and powder bed fusion in additive manufacturing (AM)10. Unfortunately, these processes often lead to defects such as oxide film formation, hot cracking, porosity, intermetallic precipitation, high residual stresses, and dimensional distortion11. To address these issues, solid-state processing techniques have been developed, which involve material consolidation below the melting point12. Moreover, the fabrication of complex aluminum components with optimal mechanical performance remains challenging using traditional manufacturing routes13. Additive manufacturing (AM) has emerged as a promising alternative to overcome these limitations14. A variety of AM technologies are currently available15, among which three-dimensional components are built layer by layer using materials such as metals, polymers, concrete, and even biological tissues13,16. The key advantages of additive manufacturing include the ability to produce intricate geometries regardless of shape or size, enable customization without the need for dedicated molds or tooling, and significantly reduce production lead times17-19.

Recently, a rotary deposition additive manufacturing (RDAM) is a technique that sequentially bonds solid layers (plates) layer by layer, analogous to the concept of AM20. RDAM is based on the concept of Friction Stir Welding (FSW), which utilizes a rotating non-consumable tool to induce frictional heat21. The tool comprises a tool shoulder and a specialized hollow tool, where the rod material is extruded into the sheet under axial force within the hollow tool. The rotating tool then advances in the transverse direction. Friction heat generated during metal-to-metal contact is harnessed to induce severe plastic deformation in the workpiece. Due to this intense plastic deformation, the material softens and flows from the front end of the rod toward the rear22. A similar concept is employed to sequentially join multiple layers. The technology offers significant advantages including: customizable parts and products with rapid production capabilities23-25, the ability to manufacture parts with complex geometries and internal structures, high material flexibility, reduced waste, and lower tooling costs26-30.

Kiani et al.31 employed friction stir additive manufacturing (FSAM) to deposit linear and cylindrical AA6061-T6 rods in multiple layers, evaluating the effectiveness of friction stir deposition (FSD) for fabricating AA6061-T6 alloy aluminum components. The study concluded that FSAM technology with AA6061-T6 can effectively produce parts with customized properties suitable for specific applications, highlighting the critical role of process parameters in optimizing material performance. The findings support the potential of FSAM in industrial applications requiring tailored mechanical and durability properties. Chaudhary et al.32 investigated the deposition of Al 6061 alloy in multiple layers using a novel friction stir powder additive manufacturing (FSPAM) process. Microstructural examination revealed fine subgrains and uniform distribution of major alloying elements.More recently, Zhang et al.33 systematically investigated ultra-multilayer and large-scale 6061 Al alloy fabricated by RDAM and reported that solution treatment combined with single-stage and dual-stage aging improved microstructural homogeneity and significantly enhanced tensile strength, while directional differences in mechanical properties remained. Their results further demonstrated that the mechanical response of RDAM-fabricated 6061 Al is strongly dependent on the heat-treatment route and sampling orientation.

Nevertheless, the response of RDAM-fabricated 6061 Al alloy to different post-deposition heat-treatment routes remains insufficiently understood, particularly regarding the coupled evolution of microstructure, mechanical anisotropy and electrochemical corrosion behavior. In the present study, a lower-temperature solution treatment followed by dual-stage aging (480 °C/2 h + 120 °C/3 h + 155 °C/6 h) was therefore employed to investigate the microstructural, mechanical and corrosion responses of RDAM-fabricated 6061 Al alloy.

2. Materials and Methods

The 6061-T5 aluminum alloy specimens for this experiment were fabricated using an RDAM-V2 (BASICSOO®) metal printer manufactured by Basicsoo (Qingdao) Intelligent Technology Co.,Ltd. The schematic of the RDAM rotary deposition solid-phase additive manufacturing process is shown in Figure 1. All specimens were printed on a 6061-T5 aluminum alloy substrate. The raw material parameters and additive manufacturing parameters can be seen in Table 1. This experiment compares the microstructure, mechanical properties, and corrosion resistance between as-deposited and heat-treated states. The heat treatment process employs solution treatment followed by dual-stage aging, implemented as follows: 480°C solution treatment for 2h + 120°C primary aging for 3h + 155°C secondary aging for 6h. The specific heat treatment process flow diagram is shown in Figure 2.

Figure 1
Additive manufacturing equipment: (a) RDAM-V2 equipment schematic diagram of additive Manufacturing; (c) Additive manufacturing specimen.
Table 1
The raw material parameters and additive manufacturing parameters.
Figure 2
The heat treatment process curves for HT specimens.

This experiment employed a Metallographic microscope (OM, IE500M), Vickers hardness tester (HV-1000SPTA), computer-controlled electronic universal testing machine (EUT5105S), electrochemical workstation (CHI760E), and scanning electron microscope (SEM, SU1510) to characterize the microstructure and properties of RDAM 6061-T5 alloy in the heat-treated (HT) and original solution-treated (OS) conditions. Its operating parameters: 200/208/230 V AC voltage; power 2 kW, frequency 50/60 Hz. Microstructural images were captured by the IE500M metallographic optical microscope. Use Keller's reagent (ratio: H2O:HNO3:HCL:HF = 95:2.5:1.5:1.0) as a metallographic etchant to etch the surface of the sample for about 30 s. Micro-Vickers hardness testing was performed using the HV-1000SPTA micro-Vickers hardness tester with a 4.9N load maintained for 10 s. Uniaxial rod tensile tests were conducted on the EUT5105S computer-controlled electronic universal testing machine, applying a 100kN force incrementally. In the CHI760E electrochemical workstation, a 3.5 wt% NaCl corrosion solution was used. The frequency parameter range for EIS curves was set between 10 ~106 Hz, while the scanning rate for Tafel curves was set at 0.01 V/s. Using a SEM scanning electron microscope with an acceleration voltage of 15 kV, observations were made of the fracture surface morphology and microstructure of the samples.

The specimen dimensions for tensile mechanical property testing in this experiment were designed according to GB/T 228.1-2021(in China) “Metallic Materials-Tensile Testing-Part 1: Method of Test at Room Temperature” (see Figure 3). Original Depositional State (OS) and Heat-Treated (HT) Actual Tensile Specimen Diagram (see Figure 4). The test material was obtained in two ways: one along the Z-axis direction, perpendicular to the printing direction (see Figure 5a), and the other along the printing direction (see Figure 5b). This study investigates the tensile properties of RDAM solid-phase additive 6061 aluminum alloy under different orientations and heat treatment processes.

Figure 3
Tensile apecimens design drawing for RDAM produced 6061 aluminum alloy.
Figure 4
Tensile specimens diagram for RDAM produced 6061 aluminum alloy.
Figure 5
Cutting position for OS and HT tensile specimens: (a) the Z-axis direction; (b) the printing direction.

3. Results and Discussion

3.1. Microstructures

Figure 6 shows the metallographic specimen sampling diagram. This experiment investigates different heat treatment processes and specimen locations as starting points, comparing the upper surface and side surfaces of specimens after rotary deposition solid-state additive manufacturing (RDAM), as illustrated in Figure 3. The top surface is perpendicular to the Z-axis along the deposition direction, primarily investigating microstructural properties parallel to the RDAM dimension. The side surface is perpendicular to the deposition direction along the Z-axis, primarily examining microstructural properties during the deposition process. Figure 7 shows microstructural characterization of the upper surface and as-deposited upper surface of 6061 aluminum alloy specimens manufactured via the RDAM process under the heat treatment parameters: 480°C solution treatment for 2h + 120°C primary aging for 3h + 155°C dual-stage aging for 6h. Figures 7a, 7b, and 7c present metallographic and SEM characterization of the as-deposited specimen upper surface; Figures 7d, 7e, and 7f show metallographic and SEM characterization of the specimen upper surface after 480°C solution treatment for 2h + 120°C primary aging for 3h + 155°C dual-stage aging for 6h.

Figure 6
Metallographic specimen sampling diagram for OS and HT processes.
Figure 7
Microstructural characterization of the upper surface of OS and HT specimens.

Figure 7 reveals that during single-layer deposition, the deposited material (rod-shaped) undergoes intense friction with the substrate or preceding layer due to the high-speed rotation and axial pressure of the rotating tool. This generates significant frictional heat, raising the temperature of the contact area above its recrystallization temperature but consistently below its melting point. The material exists in a thermoplastic state, undergoing plastic flow and dynamic recrystallization to achieve metallurgical bonding rather than melting and solidification. Due to these solid-phase deposition characteristics, the deposited layer surface exhibits a regular, continuous, grooved morphology with rotational texture determined by the rotational tool's trajectory. Additionally, gaps, voids, and cracks accompany the alloy material interfaces, as shown in Figure 7a.

As observed in Figure 7c, the deposited matrix primarily consists of supersaturated α-Al solid solution. After the two-stage aging process (Figures 7d, 7e, 7f), the alloy's grain size becomes fine and uniform, with discontinuously distributed equilibrium β-Mg2Si phases forming at grain boundaries might be alongside trace coarse Fe/Mn-containing impurity phases. Although nanoscale metastable β" strengthening phases (Mg2Si) and GP zones cannot be directly resolved under the current OM and SEM magnifications, their dense precipitation within the α-Al matrix is highly inferred based on the significant enhancement in mechanical properties discussed in the following sections. Extensive studies1,34 have rigorously confirmed that similar low-temperature pre-aging and high-temperature aging in 6061 alloys promote such high-density β" phase precipitation. Consequently, the observed peak strength is primarily attributed to this inferred β" phase dislocation pinning.

Figure 8 shows the side view of a 6061 aluminum alloy specimen manufactured using the RDAM rotary deposition solid-state additive manufacturing process under the heat treatment parameters of 480°C solution treatment for 2h + 120°C primary aging for 3h + 155°C dual-stage aging for 6h, along with the metallographic microstructure characterization of the specimen's deposited side. Figure 8a presents the metallographic characterization of the specimen's deposited side. Figure 8b shows the metallographic microstructure of the specimen side after the heat treatment process of 480°C solution treatment for 2h + 120°C primary aging for 3h + 155°C dual-stage aging for 6h. As a result, Figure 8 reveals that during the deposition process, gaps between each layer are observable, and the deposition trajectory is clearly visible around these gaps in the as-deposited specimen (see Figure 8a). Following heat treatment, the trajectory disappears due to the precipitation of strengthening phases and grain refinement recrystallization (see Figure 8b), with high-density precipitation of strengthening phases.

Figure 8
SEM of OS and HT specimen cross-sections.

3.2. XRD analysis

To further investigate the phase composition and crystallographic orientation evolution of the RDAM 6061 aluminum alloy, X-ray diffraction (XRD) analysis was performed on both the as-deposited and heat-treated specimens, as illustrated in Figure 9. The XRD patterns reveal that all specimens, regardless of their state or sampling direction, are primarily composed of the face-centered cubic (FCC) α-Al solid solution phase. Characteristic diffraction peaks corresponding to the (111), (200), (220), (311), and (222) crystal planes of α-Al are clearly identified. Notably, no distinct diffraction peaks for secondary precipitates, such as the equilibrium β-Mg2Si or metastable β″ phases, were detected in either the OS or HT states. This absence in the XRD spectra is attributed to their nanoscale dimensions and relatively low volume fraction within the α-Al matrix, which fall below the detection limit of conventional XRD, further corroborating the earlier microstructural observations.

Figure 9
X-ray diffraction (XRD) patterns of the RDAM produced 6061 aluminum alloy under OS (as-deposited) and HT (heat-treated) conditions for both upper surface and side view.

While the phase composition remains predominantly α-Al, the relative intensities of the diffraction peaks exhibit remarkable changes following the heat treatment, indicating a significant evolution in crystallographic texture. In the as-deposited (OS) state, both the upper surface and side view exhibit relatively strong (111) and (220) diffraction peaks. This specific preferred orientation is a characteristic deformation texture induced by the severe plastic deformation, high-speed rotation, and axial pressure exerted during the solid-phase deposition process of RDAM. However, after the specimens were subjected to the 480 °C/2 h solution treatment followed by the dual-stage aging process, the intensity of the (200) peak increased dramatically, becoming the dominant peak, while the intensity of the (220) peak was substantially reduced. This dramatic shift in peak intensities indicates that extensive dynamic recrystallization and grain reorientation occurred during the high-temperature solution treatment , effectively eliminating the severe processing traces and preferred orientation inherent to the as-deposited condition. This microstructural homogenization and grain refinement through recrystallization play a crucial role in the subsequent enhancement of both mechanical properties and corrosion resistance.

3.3. Hardness analysis

Based on the above analysis, the microstructure of the alloy has undergone significant changes. Therefore, analyzing the hardness distribution of the alloy to understand the relationship between microstructural changes and heat treatment processes is of great significance. The hardness distribution on the surface of the 6061-T5 aluminum alloy is shown in Figure 10. During the hardness testing process, both the upper surface and the side surface of the specimen were studied and analyzed.

Figure 10
Hardness distribution of alloys under OS and HT for RDAM produced 6061 aluminum alloy.

This experiment systematically compared the hardness of heat-treated specimens with that of as-processed, as-deposited aluminum alloy specimens. It revealed the dimensions through which heat treatment processes influence mechanical properties, demonstrating that heat treatment is a key factor in enhancing aluminum alloy hardness. As shown in Figure 10, the hardness comparison between OS and HT specimens indicates that the average hardness of specimens subjected to the heat treatment process (480°C solution treatment for 2h (water quenched) + 120°C primary aging for 3h with air cooling) + 155°C dual-stage aging for 6h with air cooling) exhibited higher values compared to the average hardness of as-processed specimens (OS). This increase was evident in both the average surface hardness and the average edge hardness of the specimens. The average surface hardness of the as-deposited (OS) specimens was 54.55 HV, while the average edge hardness was 52.42 HV. The average hardness value on the upper surface of the heat-treated specimen (HT) reached 57.3 HV, representing an increase of approximately 5.04% compared to the average hardness of the upper surface of the as-deposited specimen (OS). The average hardness value on the side surface of the heat-treated specimen (HT) reached 55.67 HV, showing an increase of approximately 6.2% compared to the average hardness of the side surface of the as-deposited specimen (OS).

During the solution treatment of heat-treated specimens, since 480°C falls below the recommended solution treatment temperature range for 6061 aluminum alloy, this temperature may be insufficient to fully dissolve the existing strengthening phases present in the as-cast T5 condition. Even with an extended holding time of 2h, dissolution may remain incomplete. In primary aging treatment, 120°C represents a relatively low temperature. At this temperature, the primary formations are atomic clusters and GP zones. These structures themselves offer limited strengthening effects but provide nucleation sites for subsequent precipitation. The secondary aging temperature of 155°C is sufficient for β'' phase formation but falls below typical peak aging temperatures. Consequently, the low temperatures during solution treatment and dual-stage aging failed to effectively relieve residual stresses in the material and did not fully precipitate strengthening phases. This results in post-heat-treated specimens exhibiting increased hardness compared to the untreated as-machined state, though the improvement is limited34. This indicates that the current heat treatment process promotes the precipitation of strengthening phases to a certain extent. However, according to precipitation hardening theories in 6xxx series alloys34, the suboptimal solid solution temperature and relatively low aging temperature theoretically restrict the full development and optimal distribution of nano-precipitates. Consequently, the material property enhancement is constrained, which is consistent with the limited hardness improvement observed in our tests. Furthermore, while the as-deposited (OS) state typically harbors microstructural instabilities and potential residual stresses due to the severe plastic deformation inherent in RDAM, the employed heat treatment conditions may theoretically be insufficient to fully relieve them. The .mechanical response after aging is consistent with enhanced precipitation strengthening by fine Mg–Si-rich metastable precipitates, likely including β″-type phases. However, because these nanoscale precipitates cannot be directly resolved by the present OM, SEM or XRD characterization, their exact phase identity requires further confirmation by TEM.

In summary, the hardness of heat-treated specimens (HT) showed a limited increase compared to as-deposited specimens (OS). This indicates that while the current heat treatment process has optimized microstructural stability and promoted the formation of strengthening phases to some extent, insufficient solution treatment temperature and low dual-stage aging temperatures resulted in incomplete precipitation of strengthening phases and incomplete release of residual stresses, thereby limiting hardness improvement. These results indicate that controlling the temperature and duration of solution treatment and aging treatment are critical factors influencing the hardness of 6061-T5 aluminum alloy.

3.5. Tensile properties

The tensile stress-strain curves of the as-deposited and heat-treated RDAM 6061 aluminum alloy specimens are presented in Figure 11, while the corresponding tensile strength and elastic modulus values obtained from three parallel specimens for each condition are summarized in Table 2. The tensile strength of the heat-treated specimen (HT) significantly increased compared to the as-deposited specimen (OS). Furthermore, the tensile strength along the X-axis (deposition printing direction) was higher than that along the Z-axis (longitudinal stacking direction), indicating superior mechanical properties. Under the heat treatment parameters of 480°C solution treatment for 2h + 120°C primary aging for 3h + 155°C dual-stage aging for 6h, the average tensile strength of the 6061 aluminum alloy specimen sampled along the X-axis (HT-X) produced by the RDAM rotary deposition solid-phase additive manufacturing process was 385.067 MPa. It is higher than the average tensile strength (222.331 MPa) of specimens sampled along the Z-axis after heat treatment (HT). The average tensile strength of specimens sampled along the X-axis in the as-deposited state (OS) was 211.576 MPa, higher than that of specimens sampled along the Z-axis in the as-deposited state (OS) (129.644 MPa). In summary, specimens processed under the heat treatment regimen of 480°C solution treatment for 2h + 120°C primary aging for 3h + 155°C dual-stage aging for 6h exhibited higher tensile strength than as-deposited specimens. Furthermore, specimens cut along the X-axis (along the deposition printing direction) demonstrated superior tensile strength compared to those cut along the Z-axis (along the stacking direction). This demonstrates that heat treatment enhances the material's tensile strength, with mechanical properties along the deposition direction outperforming those along the stacking direction.A similar directional dependence has also been reported for ultra-multilayer RDAM-fabricated 6061 Al alloy, where the interlayer interfaces and anisotropic thermo-mechanical history were considered important contributors to the lower load-bearing capacity along the build direction33.

Figure 11
Tensile Curves of OS and HT for RDAM produced 6061 aluminum alloy.
Table 2
The result analysis of tensile properties of OS and HT Specimens.

However, it should be noted that the significant increase in tensile strength is accompanied by a reduction in elongation, exhibiting a typical strength-ductility trade-off. This reduction in ductility is primarily attributed to the dense precipitation of nano-scale β" phases, which strongly pin dislocation slip during plastic deformation. While this Orowan strengthening mechanism drastically improves the ultimate tensile strength, it simultaneously restricts the material's capacity for plastic flow. Additionally, the precipitation of equilibrium phases at grain boundaries may induce micro-stress concentrations, further contributing to the decreased elongation.

3.4 Fracture Surface Analysis

The tensile fracture morphology of 6061 aluminum alloy specimens manufactured via the RDAM rotary deposition solid-state additive manufacturing process under heat treatment parameters is shown in Figure 12. The fracture morphology of the as-deposited specimen cut along the X-axis deposition direction (OS) is shown in Figures 12a and 12b; the fracture morphology of the as-deposited specimen cut along the Z-axis deposition direction (OS) is shown in Figures 12c and 12d. The fracture morphology of the heat-treated specimen cut along the X-axis deposition direction (HT) is shown in Figures 12e and 12f. The fracture morphology of the heat-treated specimen cut along the Z-axis deposition direction (HT) is shown in Figures 12g and 12h.

Figure 12
Fracture surface morphology of OS and HT specimens: (a) and (b) show OS-X fracture surfaces; (c) and (d) show OS-Z fracture surfaces; (e) and (f) show HT-X fracture surfaces; (g) and (h) show HT-Z fracture surfaces.

After heat treatment, the fracture surfaces of specimens in all orientations transformed from the mixed morphology (toughening pits + localized cleavage/intergranular) that may occur in the as-cast state to a fully toughening-pit morphology. This effectively improved interlamellar bonding, homogenized the precipitation phases, eliminated localized brittle zones, and significantly enhanced overall plasticity, as shown in Figures 12b, 12d, 12f, 12h. The post-heat-treatment fracture morphology resulted from mixed fracture, characterized by abundant dimples accompanied by river-like patterns, which were not prominent in the as-deposited state. However, anisotropy was not completely eliminated. Specimens sampled along the X-axis deposition direction typically exhibited the highest tensile strength after heat treatment. Heat treatment effectively mitigates severe Z-direction necking and enhances overall performance by improving interlayer quality and precipitation strengthening. As shown in Figures 12c and 12g, post-heat-treatment necking is mitigated. Nevertheless, the microstructural foundation formed in the as-cast state, particularly the grain size advantage in the X-direction, ensures specimens along the deposition direction (X-axis) still achieve optimal tensile strength performance after heat treatment.

3.6. Electrochemical corrosion analysis

To evaluate the effect of heat treatment on the corrosion resistance of 6061 aluminum alloy specimens manufactured via the RDAM rotary deposition solid-phase additive manufacturing process, we conducted Tafel polarization and AC impedance spectroscopy (EIS) tests on the alloy. The relevant test results and fitting outcomes are presented in Figure 13, Figure 14 and Table 3.

Figure 13
Tafel data plots for OS and HT specimens.
Figure 14
EIS data plots for OS and HT specimens.
Table 3
Electrochemical corrosion results of OS and HT Specimens.

Test results indicate that the alloy subjected to a heat treatment process comprising 480°C solution treatment for 2h + 120°C primary aging for 3h + 155°C dual-stage aging for 6h exhibits a higher autocorrosion potential position on the polarization curve (see Figure 13). Corrosion potential (Ecorr) comparison: HT-Upper surface (-0.50616V) > HT-Side view (-0.6197 V) > OS-Upper surface (-0.78053 V) > OS-Side view (-0.87164 V). The upper surface of specimens after dual-stage aging achieved an autocorrosion potential of -0.50616 V, significantly higher than the as-deposited state (see Table 3). Moreover, its self-corrosion current density is lower than that of the as-deposited alloy under identical conditions. After dual-stage aging treatment, the self-corrosion current on the specimen's side surface can reach a minimum of 4.5839E-8 A/cm2 (see Table 3). A lower self-corrosion current indicates greater corrosion resistance, demonstrating that dual-stage aging treatment significantly enhances the alloy's corrosion resistance. Corrosion potential (Ecorr) is a key parameter for assessing a material's corrosion tendency, and a higher absolute value indicates a more pronounced corrosion tendency35. The alloy subjected to dual-stage aging exhibited a higher self-corrosion potential of -0.50616 V, indicating reduced corrosion tendency. Concurrently, the lower corrosion current density of 4.5839E-8 further confirms the positive effect of dual-stage aging on enhancing the alloy's corrosion resistance. The impedance curve exhibits a semicircular feature characteristic of a capacitive loop, with the polarization resistance showing an upward trend manifested as an enlargement of the semicircle diameter36. A distinct passivation plateau was observed in both the as-deposited and dual-stage aged specimens, indicating that a protective oxide film can form on the alloy surface during corrosion, thereby enhancing its corrosion resistance. AC impedance testing further confirms that dual-stage aging treatment significantly improves the alloy's corrosion resistance. The upper surface and side of dual-stage aged specimens exhibit larger capacitive arc resistance radii. For instance, the impedance values of the HT-Upper surface and HT-Side view specimens are 40100Ω and 17850 Ω, respectively, markedly higher than the 10030 Ω and 5060 Ω values of the as-deposited specimens.

4. Conclusion

This paper presents comprehensive and in-depth testing and analysis of 6061 aluminum alloy processed via Rotary Deposition Additive Manufacturing (RDAM) and subjected to a heat treatment sequence of 480°C solution treatment for 2h + 120°C primary aging for 3h + 155°C dual-stage aging for 6h. The study examines its microstructure and properties, yielding the following conclusions:

  1. The study suggests that the α-Al matrix has β-strengthening phases and a bit of evenly spread β' phase, which makes the matrix tougher. The equilibrium phases at the grain boundaries help stop intergranular corrosion and get rid of layering that happens during deposition. Dynamic recrystallization makes the grains finer, cutting down on tiny voids and cracks and making the structure more uniform.

  2. The hardness and tensile strength of the RDAM 6061 aluminum alloy significantly increased: The upper surface hardness reached 57.30 HV, a 5.04% increase from the as-deposited state (54.55 HV), while the side surface hardness reached 55.67 HV, a 6.20% increase from the as-deposited state (52.42 HV). Simultaneously, tensile strength in the X-direction (deposition direction) reached 385 MPa, an 82% increase over the as-deposited state (212 MPa). The fracture pattern transformed from quasi-cleavage fracture in the as-deposited state to uniform, fine ductile dimples with significantly increased density. This synergistic strengthening is attributed to the high-density β" phase precipitation effectively impeding dislocation motion and inhibiting crack propagation, thereby enhancing mechanical properties.

  3. The corrosion resistance of RDAM 6061 aluminum alloy significantly improved: the self-corrosion potential on the upper surface reached -0.50616 V, and the self-corrosion current density on the side surface was 4.5839 × 10−8 A/cm2, demonstrating markedly enhanced corrosion resistance compared to the as-deposited state. This improvement is attributed to the dual-stage aging treatment, which significantly strengthened the matrix and formed equilibrium phases at grain boundaries. This effectively suppressed intergranular corrosion and grain boundary propagation, achieving synergistic enhancement of corrosion resistance and mechanical properties.

5. Data Availability

The data that support the findings of this study are available from the corresponding author upon reasonable request.

6. References

  • 1 Engler O, Marioara CD, Aruga Y, Kozuka M, Myhr OR. Effect of natural ageing or pre-ageing on the evolution of precipitate structure and strength during age hardening of Al-Mg-Si alloy AA 6016. Mater Sci Eng A. 2019;759:520-9. https://doi.org/10.1016/j.msea.2019.05.073
    » https://doi.org/10.1016/j.msea.2019.05.073
  • 2 Hirsch J, Al-Samman T. Superior light metals by texture engineering: optimized aluminum and magnesium alloys for automotive applications. Acta Mater. 2013;61(3):818-43. https://doi.org/10.1016/j.actamat.2012.10.044
    » https://doi.org/10.1016/j.actamat.2012.10.044
  • 3 Zainelabdeen IH, Al-Badour FA, Adesina AY, Suleiman R, Ghaith FA. Friction stir surface processing of 6061 aluminum alloy for superior corrosion resistance and enhanced microhardness. Int J Lightw Mater Manuf. 2023;6(1):129-39. https://doi.org/10.1016/j.ijlmm.2022.06.004
    » https://doi.org/10.1016/j.ijlmm.2022.06.004
  • 4 Devaraju A, Kumar A, Kotiveerachari B. Influence of addition of Grp/Al2O3p with SiCp on wear properties of aluminum alloy 6061-T6 hybrid composites via friction stir processing. Trans Nonferrous Met Soc China. 2013;23(5):1275-80. https://doi.org/10.1016/S1003-6326(13)62593-5
    » https://doi.org/10.1016/S1003-6326(13)62593-5
  • 5 Adin MŞ. Machining aerospace aluminium alloy with cryo-treated and untreated HSS cutting tools. Adv Mater Process Technol. 2024;10(3):2664-89. https://doi.org/10.1080/2374068X.2023.2273035
    » https://doi.org/10.1080/2374068X.2023.2273035
  • 6 Adin MS, Okumus M. Investigation of microstructural and mechanical properties of dissimilar metal weld between AISI 420 and AISI 1018 steels. Arab J Sci Eng. 2022;47(7):8341-50. https://doi.org/10.1007/s13369-021-06243-w
    » https://doi.org/10.1007/s13369-021-06243-w
  • 7 Aruri D, Adepu K, Adepu K, Bazavada K. Wear and mechanical properties of 6061-T6 aluminum alloy surface hybrid composites [(SiC+Gr) and (SiC+Al2O3)] fabricated by friction stir processing. J Mater Res Technol. 2013;2(4):362-9. https://doi.org/10.1016/j.jmrt.2013.10.004
    » https://doi.org/10.1016/j.jmrt.2013.10.004
  • 8 Kheirkhah S, Imani M, Aliramezani R, Zamani MH, Kheilnejad A. Microstructure, mechanical properties and corrosion resistance of Al6061/BN surface composite prepared by friction stir processing. Surf Topogr. 2019;7(3):035002. https://doi.org/10.1088/2051-672X/ab2a4b
    » https://doi.org/10.1088/2051-672X/ab2a4b
  • 9 Galy C, Le Guen E, Lacoste E, Arvieu C. Main defects observed in aluminum alloy parts produced by SLM: from causes to consequences. Addit Manuf. 2018;22:165-75. https://doi.org/10.1016/j.addma.2018.05.005
    » https://doi.org/10.1016/j.addma.2018.05.005
  • 10 Dadbakhsh S, Hao L, Jerrard PGE, Zhang DZ. Experimental investigation on selective laser melting behaviour and processing windows of in situ reacted Al/Fe2O3 powder mixture. Powder Technol. 2012;231:112-21. https://doi.org/10.1016/j.powtec.2012.07.061
    » https://doi.org/10.1016/j.powtec.2012.07.061
  • 11 Zhiguang Z, Zhiheng H, Li SH, Tingting L, Wenhe L, Upadrasta R, et al. Recent progress on the additive manufacturing of aluminum alloys and aluminum matrix composites: microstructure, properties, and applications. Int J Mach Tools Manuf. 2023;190:104047.
  • 12 Palanivel S, Nelaturu P, Glass B, Mishra RS. Friction stir additive manufacturing for high structural performance through microstructural control in an Mg based WE43 alloy. Mater Des. 2014;65:934-52.
  • 13 Srivastava M, Rathee S. Microstructural and microhardness study on fabrication of Al 5059/SiC composite component via a novel route of friction stir additive manufacturing. Mater Today Proc. 2021;39:1775-80. https://doi.org/10.1016/j.matpr.2020.07.137
    » https://doi.org/10.1016/j.matpr.2020.07.137
  • 14 Zhang M, Jiang T, Xie Y, Feng X, Su Y, Shen Z, et al. Microstructure evolution and strengthening mechanisms of an additive friction stir deposited multi-layer Al-Mg-Sc-Zr alloy. J Alloys Compd. 2024;1004:175783.
  • 15 Zhao N, Parthasarathy M, Patil S, Coates D, Myers K, Zhu H, et al. Direct additive manufacturing of metal parts for automotive applications. J Manuf Syst. 2023;68:368-75.
  • 16 Ahmed MMZ, El-Sayed Seleman MM, Elfishawy E, Alzahrani B, Touileb K, Habba MIA. The effect of temper condition and feeding speed on the additive manufacturing of AA2011 parts using friction stir deposition. Materials (Basel). 2021;14(21):6396.
  • 17 Bandyopadhyay A, Traxel KD, Lang M, Juhasz M, Eliaz N, Bose S. Alloy design via additive manufacturing: Advantages, challenges, applications and perspectives. Mater Today. 2022;52:207-24.
  • 18 Vimal KEK, Naveen Srinivas M, Rajak S. Wire arc additive manufacturing of aluminium alloys: a review. Mater Today Proc. 2021;41:1139-45.
  • 19 Colorado HA, Gutierrez-Velasquez EI, Gil LD, Camargo IL. Exploring the advantages and applications of nanocomposites produced via vat photopolymerization in additive manufacturing: a review. Adv Compos Hybrid Mater. 2024;7(1):1.
  • 20 Rishabh D, Rakesh KS, Sanjay K, Ashish KS. Parametric optimization of process parameters during the friction stir processing of Al7075/SiC/waste eggshell surface composite %. Mater Today Proc. 2021;47(P13):3884-90.
  • 21 Kumar S, Srivastava AK, Singh RK. Fabrication of AA7075 hybrid green metal matrix composites by friction stir processing technique %. Ann Chim. 2020;44(4):295-300.
  • 22 Srivastava AK, Maurya M, Saxena A, Maurya NK, Dwivedi SP, Dixit AR. Microstructural and fractographic analysis of A359/Si3N4 surface composite produced by friction stir processing. Int J Mater Res. 2021;112(1):68-77.
  • 23 Leong KF, Teng PSP, Er BH, Tee CH. Mass customization and testing of braces using additive manufacturing. Mater Today Proc. 2022;70:593-8. https://doi.org/10.1016/j.matpr.2022.09.609
    » https://doi.org/10.1016/j.matpr.2022.09.609
  • 24 Patel P, Gohil P. Custom orthotics development process based on additive manufacturing. Mater Today Proc. 2022;59:A52-63. https://doi.org/10.1016/j.matpr.2022.04.858
    » https://doi.org/10.1016/j.matpr.2022.04.858
  • 25 Lazorenko G, Kasprzhitskii A. Geopolymer additive manufacturing: a review. Addit Manuf. 2022;55:102782. https://doi.org/10.1016/j.addma.2022.102782
    » https://doi.org/10.1016/j.addma.2022.102782
  • 26 Druzgalski CL, Ashby A, Guss G, King WE, Roehling TT, Matthews MJ. Process optimization of complex geometries using feed forward control for laser powder bed fusion additive manufacturing. Addit Manuf. 2020;34:101169.
  • 27 Salmi M. Comparing additive manufacturing processes for distributed manufacturing. IFAC-PapersOnLine. 2022;55(10):1503-8.
  • 28 Colorado HA, Velásquez EIG, Monteiro SN. Sustainability of additive manufacturing: the circular economy of materials and environmental perspectives. J Mater Res Technol. 2020;9(4):8221-34.
  • 29 Javaid M, Haleem A, Singh RP, Suman R, Rab S. Role of additive manufacturing applications towards environmental sustainability. Adv Ind Eng Polym Res. 2021;4(4):312-22.
  • 30 Belhadi A, Kamble SS, Venkatesh M, Chiappetta Jabbour CJ, Benkhati I. Building supply chain resilience and efficiency through additive manufacturing: an ambidextrous perspective on the dynamic capability view. Int J Prod Econ. 2022;249:108516.
  • 31 Kiani S, Mirsalehi SE, Sahraei A. Linear and cylindrical friction stir additive manufacturing (FSAM) of AA6061-T6 by consumable rods: metallurgical structure, wear, and corrosion properties. Weld World. 2024;68(11):2869-89.
  • 32 Chaudhary B, Jain NK, Murugesan J, Patel V. Exploring temperature-controlled friction stir powder additive manufacturing process for multi-layer deposition of aluminum alloys. J Mater Res Technol. 2022;20:260-8.
  • 33 Zhang R, Jiang Z, Yang L, Fang J, Liu P. Effects of heat treatment on the microstructures and mechanical properties of ultra-multilayer and large-scale 6061 aluminum alloy fabricated by rotational deposition additive manufacturing (RDAM). Weld World. 2026.
  • 34 Yao SJ, Tang QH, Yang J, Wang CY, Sun HF, Rong RL, et al. Microstructural characterization and mechanical properties of 6061 aluminum alloy processed with short-time solid solution and aging treatment. J Alloys Compd. 2023;960:170704.
  • 35 Bao WZ, Xiang T, Chen L, Du P, Zhang ZW, Xie GQ. Corrosion behavior of high-performance crystalline CuCrZr/amorphous CuZrAl composites in NaCl solution. J Mater Res Technol. 2022;21:5004-17.
  • 36 Zhang XM, Xiong S, Gao F, Du JY, Du QJ. Preparation and tribological properties of SiO/WO nanocomposite lubricant. Ind Lubr Tribol. 2023;75(1):60-6.

Associate Editor:

Ana Sofia de Oliveira.

Editor-in-Chief:

Luiz Antonio Pessan.

Publication Dates

  • Publication in this collection
    16 Nov 2026
  • Date of issue
    2026

History

  • Received
    22 Dec 2025
  • Reviewed
    12 July 2026
  • Accepted
    23 Sept 2026
location_on
ABM, ABC, ABPol UFSCar - Dep. de Engenharia de Materiais, Rod. Washington Luiz, km 235, 13565-905 - São Carlos - SP- Brasil. Tel (55 16) 3351-9487 - São Carlos - SP - Brazil
E-mail: pessan@ufscar.br
rss_feed Stay informed of issues for this journal through your RSS reader
Go to top