Abstract
This study investigates alkali-activated cements (AAC), comprising blast furnace slag (BFS) along with industrial by-products like rice husk ash (RHA) and metakaolin (MK), activated by sodium hydroxide (NaOH). The aim is to assess the impact of SiO2/Al2O3 and CaO/SiO2 ratios on AAC's mechanical strength and hydrated compounds. Mechanical and microstructural tests were carried out. Compositions with a CaO/SiO2 ratio near 1 exhibited superior mechanical strength, approximately 35–40 MPa at 28 days, while the SiO2/Al2O3 ratio did not significantly affect the outcomes. X-ray diffraction and thermal analysis revealed the formation of hydrated calcium silicate (CSH) and hydrotalcite as hydrated compounds. This suggests that BFS can enhance AAC results. In conclusion, CaO/SiO2 ratios play a crucial role in influencing the strength gains of AAC. Verifying the influence of these relationships can contribute to the study of dosage and understanding of hydration processes.
Keywords:
alkali activated cement; slag; rice husk ash; CaO/SiO2; SiO2/Al2O
Resumo
Este estudo investiga cimentos ativados alcalinamente (CAA), compostos por escória de alto-forno (EAF) juntamente com cinza de casca de arroz (CCA) e metacaulim (MK), ativados por hidróxido de sódio (NaOH). O objetivo é avaliar o impacto das relações SiO2/Al2O3 e CaO/SiO2 na resistência mecânica e nos compostos hidratados do CAA. Ensaios mecânicos e microestruturais foram realizados. Composições com uma razão CaO/SiO2 próxima de 1 apresentaram resistência mecânica superior, aproximadamente 35 a 40 MPa aos 28 dias, enquanto a razão SiO2/Al2O3 não afetou significativamente os resultados. A difração de raios-X e a análise térmica revelaram a formação de silicato de cálcio hidratado (CSH) e hidrotalcita como compostos hidratados. Isso sugere que a EAF pode aprimorar os resultados do CAA. Em conclusão, as razões CaO/SiO2 desempenham um papel crucial na influência dos ganhos de resistência do CAA. Verificar a influência dessas relações podem contribuir para o estudo de dosagem e compreensão dos processos de hidratação.
Palavras-chave:
cimento álcali-ativado; cinza da casca de arroz; CaO/SiO2; SiO2/Al2O
1 INTRODUCTION
Aiming at reducing carbon dioxide (CO2) emissions, studies involving cement with or without clinker content combined with the use of industrial residues have been developed in recent years. In this context, aluminous, sulfo-aluminous, supersulfated and alkali-activated cements (AAC) arise [1], [2].
Alkali-activated cements (AAC) basically use by-products or industrial residues as raw materials, such as fly ash, blast furnace slag, and metakaolin, a primary product produced by an industrial process. These materials are rich in alumina (Al2O3), silica (SiO2), and calcium oxide (CaO), which, when activated by an alkaline solution, react with each other and form the CSH gel as the main product of the hydration reaction or the CASH gel, hydrated calcium silicate modified by Al [1]. On the other hand, geopolymers are classified as a subgroup of AAC, as they form alkaline systems rich in SiO2 and Al2O3 from materials such as ash, metakaolin, and clay. This system, when activated, develops as a product of the hydrated aluminum-silicate reaction (NASH) [3], [4].
In addition to the low environmental impact, AAC has other advantages when compared to Portland cement, such as the potential for greater compressive strength and low heat of hydration. However, these characteristics can be affected depending on the chemical composition of the raw materials used, the curing conditions and the fineness of the material [5].
Some studies that investigated different chemical compositions of the slag in the production of AAC, it was found that higher levels of magnesium oxide (MgO) in its composition result in greater resistance to compression and the formation of hydrotalcite. Raw materials with higher Al2O3 concentration, on the other hand, presented lower heat of hydration and no influence on strength, in addition to higher Al contents in the CSH gel [6], [7].
Nazari et al. [8], Kusbiantoro et al. [9], Hwang and Huynh [10], Sturm et al. [11], Nimwinya et al. [12], Sore et al. [13], Darsanasiri et al. [14], Shaswat et al. [15] have studied alkali-activated cements based on other pozzolans such as rice husk ash (RHA) in their composition. The results obtained show the formation of new mineral phases and an improvement of the mechanical strength with the addition of rice husk ash and with curing temperature. High SiO2/Al2O3 ratios required high curing temperatures to improve the degree of polymerization and mechanical strength.
Rice husk is an abundant material in rice producing countries such as China, India, and Brazil. Rice husk is rich in silica (SiO2) and comes from the processing of rice grains for food consumption. Using the ash from this burning process for energy generation has become an environmental problem [16]. It is estimated that the world production of rice is 600 million tons, 20% of which is husk, totaling 120 million tons per year [17]. Data from 2022 shows that Brazil's production is about 10.8 million tons of paddy rice per year. Brazil is considered one of the largest rice producers in the world, and the southern region of the country is responsible for most of the production [18].
The use of rice husk ash (RHA) as an amorphous silica in addition to cement has been studied since 1960, when the first patents appeared [16]–[18]. The first records of studies carried out on rice husk ash were from Mehta, who obtained a patent in 1973 for his study related to the pozzolanic reactivity of RHA [19]. In 1976, another patent obtained by Pitt was related to the form of combustion of rice husks [20]. Since then, other studies have followed, such as Zain et al. [19] and Hoppe Filho et al. [21], who studied the production and reactivity of RHA.
The use of RHA as a partial replacement for Portland cement has become an alternative in favor of sustainability [22], [23]. When added to concrete in partial replacement of Portland cement in percentages from 15% to 35%, there may be an improvement in compressive strength. The use of RHA to improve the properties of concrete has also been studied: workability [24], [25], durability by attacking sulfates [22], penetration by chloride ions [26] and electrical resistivity [27]. As it is an extremely thin material, RHA requires greater consumption of water and has high cohesion [28]. In addition, RHA is introduced between the cement grains and modifies the microstructure of the system, reducing free spaces for water and consequently decreasing drying shrinkage [29], [30].
Concerning low environmental impact cements, RHA was incorporated into geopolymers [12], [13] and good results were obtained. However, there was a need for large amounts of alkaline activator and thermal cure at high temperatures (60°C to 90°C). Nimwinya et al. [12] and Sore et al. [13] also verified the influence of the relationship between silica and alumina (SiO2/Al2O3) (2,0 to 5,0), which, when combined with adequate thermal curing conditions, improved the compressive strength of geopolymers, forming a denser and more homogeneous structure [8]–[12].
Longhi et al. [31], aiming at the valorization of kaolin sludge for the production of geopolymers, used an SiO2/Al2O3= 4 ratio and achieved compressive strength results of 75 MPa on the third day, although at 90 days it presented a reduction of 14%. This fact can be explained by the greater amount of soluble silicates in the geopolymer composition.
RHA, rich in silica, together with calcium oxide present in pozzolans, are basic components for the formation reaction of the CSH compound responsible for the development of the mechanical strength of cement [32]. Studies analyzing the CaO/SiO2 ratio in the composition of the AACs refer only to the characterization of the slags in terms of their degree of hydraulicity and basicity [33]. Thus, rice husk ash appears as an alternative source of silica in addition to traditional cement and AAC, given the improvement in the mechanical properties of these materials [32]. Thus, this work proposed the development of an AAC focusing on evaluating the influence of the CaO/SiO2 and SiO2/Al2O3 ratios of the precursors on the mechanical and microstructural properties of the AAC.
2 MATERIALS AND EXPERIMENTAL PROGRAM
2.1 Materials
To carry out this study, two types of slag were used: slag (A) from charcoal ovens and slag (B) from coke ovens. These materials were dried for 24 hours in an oven at 105°C and after they were powered in a ball mill for 3 hours until reaching the desired fineness, similar to that of conventional cement (around 450 g/cm2). The metakaolin (MK) used was a commercial product of a national company. Rice husk ash (RHA) was supplied by a national manufacturer as a commercial material produced by a fluidized bed combustion system. The alkaline activator defined for use in this work was sodium hydroxide (NaOH). The activator is a commercial product from the brand Sodabel 99 in scales.
2.1.1 Material characterization
The chemical compositions of materials obtained by X-Ray fluorescence, their density and fineness are expressed in Table 1. The slag has in its composition CaO, SiO2, Al2O3 and MgO, and slag A has a lower amount of calcium and higher amounts of magnesium and alumina in its composition. In turn, metakaolin was rich in silica and alumina, and RHA indicated a predominance of SiO2 in its composition. Metakaolin had a specific surface of 1025 m2/kg and an RHA of 975 m2/kg. This shows that the materials have a similar fineness.
The laser particle size distribution of materials is shown in Figure 1 and Table 2 shows the particle size of each retained material accumulated between 50% and 90%.
Figure 2 shows the X-Ray diffraction analysis of materials in which it was observed that the slag does not present characteristic peaks, being considered an amorphous material. It is observed that MK is more crystalline with well-defined peaks and RHA is a less crystalline material with an SiO2 peak.
X-ray diffraction (XRD) of RHA, MK, Slag A and B. H (Fe2O3), C – cristobalite, K - kaolinite, M - muscovite, Q - quartz.
The diffractogram in Figure 2 indicates the presence of cristobalite peaks and a pronounced halo between 15 and 35° (2θ), indicating the presence of amorphous content for the rice husk ash. The presence of amorphous content in precursor materials influences pozzolanic activity and is fundamental in the formation of the main reaction products of alkali-activated materials, C-A-S-H gel [31].
2.2 Methods
2.2.1 Definition of compositions
The alkaline activator content (NaOH) was 5% and was based on Langaro et al. [2]. The proportion between the raw materials (RHA, MK and BFS) was based on Longhi et al. [31].
As Longhi et al. [31] applied the SiO2/Al2O3 ratio close to 4.4 for geopolymers, the same ratio was fixed to define the compositions of AAC_A_0.49 and AAC_B_0.70 in Table 3. Also, from preliminary results, it was observed that the CaO/SiO2 ratio close to 1.0 could have a positive effect ly. Thus, the AAC_A_0.97, AAC_B_1.37 AAC_B_0.90 were defined. The compositions used are shown in Table 3.
The CaO/SiO2 and SiO2/Al2O3 ratios were calculated based on the chemical composition of the materials.
2.2.2 Preparation of pastes
The water/binder ratio of 0.4. The mixing process was carried out by adding the activator to the water and mixing until it was completely dissolved. It was then added to the rest of the previously mixed materials. Then, manual mixing was performed for one minute.
2.2.3 Paste characterization
2.2.3.1 Compressive strength
For the compressive strength tests, specimens were molded with cement paste with the dimensions of 30x30x30mm and they were stored in a humidity chamber (95% humidity) at 23°C. After 48 hours, they were demolded and subjected to the same temperature and humidity conditions.
An EMIC machine (DL-30000, EMIC, Brazil) with a load application rate of 1 mm/min was used. Three specimens were made for each test at 7, 28 and 91 days.
2.2.3.2 Isothermal Conduction Calorimetry
For the calorimetry measurements, the pastes were inserted in a Calmetrix calorimeter, model I-Cal 2000 HPC, which operates with up to two samples simultaneously, and were monitored for 7 days at 23°C.
2.2.3.3 Microstructure Analysis
After compressive strength tests, part of the samples were fractured into small pieces and submerged in acetone for 2h. After this period, the acetone was removed through a buchner filter coupled to a vacuum pump and then subjected to a temperature of 40°C for 30 min in order to completely evaporate the acetone.
For the X-ray diffraction (XRD) and thermogravimetry (TG/DTG) analyses, the samples were ground into particles smaller than 150 µm. For the scanning electron microscopy (SEM), the samples were fragmented into small pieces (about 5 mm).
2.2.3.4 X-ray Diffractometry (XRD)
The X-ray diffraction analyses were performed using the Empyrean diffractometer from Panalytical with the following parameters: wavelength of 1.54 Ᾰ; sweep angles of 5° – 70° (2θ) and 0.02° pitch every 10 seconds at 7 and 28 days.
2.2.3.5 Thermogravimetric analysis (TG/DTG)
Thermogravimetric analyses (TG/DTG) were performed using the TA Instruments SDT Q600 device with the following parameters: heating range from 30°C to 900°C; heating flow 10°C min-1; inert atmosphere – nitrogen; 100mL flow min-1 at 7 and 28 days.
2.2.3.6 Scanning Electron Microscopy (SEM)
Scanning electron microscopy (SEM) provides information regarding the morphology and identification of chemical elements in the solid sample. Scanning electron microscopy assay was used for samples ground into small fragments at 28 days.
3 RESULTS AND DISCUSSIONS
3.1 Calorimetry measurements
Figure 3 shows the heat rate and total heat rate curves of hydration for the AAC pastes over the 7-day period. Note that for the AAC with slag A (AAC_A) (Figure 3b), the rate of heat released is lower than that of the AAC composed of slag B (AAC_B) (Figure 3d). It is also observed that AAC_A_0.97 presented a heat release peak before 20 hours, whereas the same is not observed for AAC_A_0.49. In addition, the total heat accumulated by AAC_A_0.97 was greater than that accumulated by AAC_A_0.49, which indicates a greater formation of hydrated compounds.
Heat rate and total heat of hydration curves for days p: AAC with CaO/SiO2 ratio 0.49 and 0.97 for slag A and 0.70, 0.90 and 1.37 for slag B.
For AAC_B_1.37 and AAC_B_0.70, there is a heat peak released before 20 hours, the second being of greater intensity. AAC_B_0.90 showed the peak of heat release between 15 and 30 hours, indicating a delay in the hydration process compared to other compositions. From 40 hours onwards, the heat release rate remained similar for all three samples.
AAC_B_0.90 showed the greatest amount of total heat released. AAC_B_0.70, on the other hand, accumulated more heat than 1.37.
The first peak in the cement system is related to the dissolution of particles and the reaction of the aluminum phase. The hydration products of AAC are CSH and CASH gel [1].
The appearance of the second peak is associated with the formation of gels due to the hydration of calcium silicate. A lower formation of calcium silicate in the slag leads to a smaller area of the second exothermic peak. Therefore, the AAC_B samples indicate a higher formation of hydrated products and consequently higher compressive strengths.
For the AAC with slag A (Figure 3a), the rate of heat release is lower than that of AAC with slag B, which may be related to the fineness of the material. The fineness of the raw material provides greater reactivity of the material, which is significant only at early ages, not significantly affecting compressive strength at 28 days. The increase in strength that occurs at the age of 28 days with the finer slag A AAC may have been due to the lower heat of hydration released, resulting in the development of a less porous microstructure [34].
3.2 X-ray diffraction
Figure 4 shows the diffractograms for the AAC pastes composed of slag A (AAC_A) and AAC pastes composed of slag B (AAC_B) (Figure 5) presented according to the CaO/SiO2 ratio and curing ages (7 and 28 days).
X-ray diffractograms (XRD) of AAC with CaO/SiO2 ratio 0.49 and 0.97 for slag A, at 7 (a) and 28 (b) days. CSH – Hydrated Calcium Silicate, CASH - Hydrated calcium aluminosilicate, HT – Hydrotalcite.
X-ray diffractograms (XRD) of AAC with CaO/SiO2 ratio 0.70; 0.90 and 1.37 for slag B, at 7 (a) and 28 (b) days. CSH – Hydrated Calcium Silicate, CASH - Hydrated calcium aluminosilicate, HT – Hydrotalcite.
It is observed that for the compositions of both AAC_A and AAC_B at all ages, there was the presence of crystalline CSH/CASH around 29°-30° 2Ө. According to the literature, alkali-activated systems are known to have CSH/CASH as their main hydration product. AAC_A_0.49 and AAC_B_0.70 and AAC_B_0.90 also showed the formation of hydrotalcite [6], [7], [25].
For the AAC_A (Figure 4) samples, it is observed that the intensity of the CSH/CASH and HT peaks formed at 28 days (Figure 4b) increased compared to 7 days (Figure 4a), which explains the increase in resistance over time.
Compositions with slag B (Figure 5) also showed formation of CSH/CASH and HT, but the latter was less evident. AAC_B_1.37 and mainly AAC_B_0.90 showed higher formation of CSH/CASH.
Samples with greater formation of CSH and lesser amount of HT can be explained by the greater incorporation of Al2O3 in the hydrated gel (CASH), as stated by Chen and Brouwers [35]. This happens in AAC_A_0.97, as the slag has a greater amount of alumina than in AAC_B_1.37. The incorporation of alumina-rich MK into compositions with slag B contributed to the formation of CASH, resulting in diffractograms with broader peaks and indicating material with more amorphous characteristics.
Chen and Brouwers [35] and Gruskovnjak et al. [36] indicate that the formation of HT still depends on the amount of Mg in the composition of the AAC, but the amount of Mg present in the slag does not have a significant difference (A=6.2% and B=4.3%). Thus it is considered that the formation of HT could be related to the amount of alumina in the slag (A=13.9% and B=8.9%).
According to Taylor [37], samples that are more amorphous have wider and less intense CSH peaks and develop greater mechanical strength.
3.3 Thermogravimetric Analysis
Figure 6 and Figure 7 show the thermogravimetric analyses according to the type of slag (A or B), CaO/SiO2 ratio and curing ages (7 and 28 days).
Thermal analysis (TG and DTG) of AAC with CaO/SiO2 ratio 0.49 and 0.97 for slag A, at 7 (a) and 28 (b) days. CSH – Hydrated Calcium Silicate, CASH - Hydrated calcium aluminosilicate, HT – Hydrotalcite
Thermal analysis (TG and DTG) of AAC with CaO/SiO2 ratio 0.70, 0.90 and 1.37 for slag B, at 7 (a) and 28 (b) days. CSH – Hydrated Calcium Silicate, CASH - Hydrated calcium aluminosilicate, HT – Hydrotalcite
In the TG/DTG curves, a peak between 50° and 200°C is observed in all samples, which refers to the loss of mass related to CSH/CASH. The HT decomposition is only identified in samples AAC_A_0.97, AAC_A_0.49 and AAC_B_1.37, with peaks at 300° and 600°C.
Mass losses in AAC_A_0.97 were greater than in AAC_A_0.49. As for AAC_B, there is a greater loss of mass related to the CSH/CASH in the dosages 0.70 and 0.90 than in the 1.37 sample, as shown by the XRD analysis. These greater mass losses are linked to the greater amount of hydrated products.
The HT decomposition phase, similarly to the XRD analyses, is clearer in the AAC_B_1.37 sample, indicating a greater amount. It is also observed that the peaks are smaller at 7 days (Figure 7a) when compared to 28 days (Figure 7b).
Thermogravimetric analysis confirms the results found in XRD, as well as other bibliographic results [6],[7] where the formation of CSH/CASH (50°-200°C) and hydrotalcite (200°-400°C) in the slag activation was also observed.
3.4 Scanning Electron Microscopy
In order to observe the hydrated compounds already identified in the previous analyses (DRX and TG), microscopy analyses (SEM) were performed.
Microscopy was performed at 28 days of age of the paste, and is presented according to the type of slag and the CaO/SiO2 ratio.
The hydrated compost (CSH/CASH) was observed in all samples of both slags, but with a different structure in each one of them (Figure 8).
Scanning electron microscopy (SEM) of AAC_A with CaO/SiO2 ratio 0.49 and 0.97, at 28 days. (a) AAC_A_0.97 (b) AAC_A_0.49. CSH – Hydrated Calcium Silicate, CASH - Hydrated calcium aluminosilicate, HT – Hydrotalcite.
In Figure 8a, the presence of CSH/CASH gel is observed with less crystalline structure, being denser and more compact. On the other hand, in Figure 8b, the formation of CSH/CASH is present in a smaller amount and with a more porous structure, which can be related to the low compressive strength. The formation of well-developed and disordered platelets characteristic of hydrotalcite is also observed in AAC_A_0.49.
Figure 9 shows the images related to AAC_B with ratios 0.70, 0.90 and 1.37.
Scanning electron microscopy (SEM) of AAC B with CaO/SiO2 ratio 0.70, 0.90 and 1.37, at 28 days. (a)(b) AAC_B_1.37 (c) AAC_B_0.70 (d) AAC_B_0.90. CSH – Hydrated Calcium Silicate, CASH - Hydrated calcium aluminosilicate, HT – Hydrotalcite.
Note that the CASH present in AAC_B has a different and more reticulated structure from that observed in AAC_A, which becomes easier to identify.
For AAC_B_1.37 represented by Figure 9a, the CASH is presented in the form of combs and with a less amorphous structure. In Figure 9b, the formation of hydrotalcite is observed, as already found in the previous analyses [38].
The images of hydrotalcite (Figure 8b and Figure 9b) observed in the SEM are consistent with the work of Pérez-Ramirez and Abelló [38].
For the other compositions with slag B (AAC_B), greater formation of CASH with a slightly more amorphous structure is identified, in the same way as AAC_A, which may have interfered to obtain higher strengths.
Figure 10 shows the EDS analyses performed on samples AAC_A, AAC_B, AAC_B_0,70 and AAC_B_0.90 at 28 days.
EDS of the AAC micrograph at 28 days. (a) AAC_A, (b) AAC_B, (c) AAC_B_0.70 and (d) AAC_B_0.90
The presence of CASH can be confirmed by the greater amount of Ca, Si and Al elements for the pastes composed of both slag A and B. Furthermore, it is observed that the points in Figure 10c and 10d show higher amounts of Al when compared to 10(b), which can be related to the incorporation of MK in the pastes (Table 4).
3.5 Compressive strength
Figure 11 shows the compressive strength values obtained for the different mixture proportions.
Compressive strength of the AACs with CaO/SiO2 ratio 0.49 and 0.97 for slag A and 0.70, 0.90 and 1.37 for slag B, at 7, 28 and 91 days.
The use of RHA and MK together with slag A (AAC_0.49) was not satisfactory, as the compressive strength decreased compared to AAC_A_0.97. This behavior can be related to the lower CSH formation and a more porous structure, which impaired the development of compressive resistance. As for the samples AAC_B_0.70 and AAC_B_0.90, the use of RHA and MK improved the compressive strength, which was related to a greater amount of CSH and a denser structure.
The graph in Figure 12 shows the compressive strength as a function of the SiO2/Al2O3 and CaO/SiO2 ratio.
Compressive strength of AAC's, with A and B slag in relation to SiO2/Al2O3 CaO/SiO2, at 28 days.
AAC_A_0.49 and AAC_B_0.70 had an SiO2/Al2O3 ratio = 4.40, but it is observed that this ratio did not have the same influence for the two slags. AAC_A_0.97 presented compressive strength values superior to the mix AAC_B_1.37, reaching 35 MPa at 28 days, while the composition AAC_B_1.37 reached only 17 MPa.
Regarding the CaO/SiO2 ratio, it is observed that the closer to 1.0, the better the compressive strength results (Figure 12).
With the addition of RHA rich in SiO2 and MK in the composition, the ratio of calcium oxide and silica for the AAC_A samples was reduced from 0.97 to 0.49, and consequently the compressive strength values dropped from 35MPa to 15 MPa at 28 days. As for the samples of AAC_B, the decrease of the CaO/SiO2 ratio from 1.37 to 0.90 and 0.70 with the incorporation of RHA favored the development of compressive resistance, obtaining values close to 40 MPa at 28 days (increase of 42.5%) for both AAC_B_0.70 and AAC_B_0.90. It is also observed that AAC_B_0.90 reached 30 MPa at 7 days, while AAC_B_0.70 obtained 13 MPa and AAC_B_1.37 reached 10 MPa.
The values obtained confirm what Frearson apud Pal et al. [33] observed, which is that the hydraulic activity increases with the increase of CaO and decreases with the increase of the silica content. In other words, when materials with a higher amount of CaO (slag B) were used, the highest mechanical strengths occurred. The addition of RHA increased the amount of silica in the composition of the AAC, which interfered with the hydraulic activity and, consequently, with the strength gain.
Table 5 presents an analysis of studies with different AAC precursors, and indicates the SiO2/Al2O3 and CaO/SiO2 ratios used.
Analysis of studies with different AAC precursors, and indicates the SiO2/Al2O3 and CaO/SiO2 ratios.
Table 5 shows that work related to alkali-activated cements has intensified in the incorporation of different residues, not only slag. Few studies accounted for the CaO/SiO2 ratio in the development of pastes; this ratio is generally used as a method of slag classification according to the basicity and hydraulicity index.
Thus, analyzing the studies presented in Table 5, it is seen that in most studies the CaO/SiO2 ratio is close to 1.0.
Darsanasiri et al. [14] on the contrary, presented a CaO/SiO2 ratio = 0.4, considerably low and even so it obtained satisfactory compressive strengths, this is due to the greater amount of alumina present in the raw material used and the high content of activator. On the other hand, Font et al. [40] the ratio of CaO/SiO2 is around 1.3, but it also presents a high level of activator and thermal cure to obtain satisfactory strengths. Shaswat et al. [15], did not indicate the chemical composition of the precursors in the work, thus, it is not possible to state which relationships were used by them, but even so, a content of 13% of alkaline activator in their compositions was observed.
4 CONCLUSIONS
In this study, the use of two slags of different chemical composition were used together with RHA and MK. From compressive strength tests and analysis of the hydration mechanisms of the AAC, it can be concluded that:
The use of RHA, rich in SiO2, as raw material for AAC has become a viable alternative when used with slag with a high content of calcium in its composition. The silica present in the ash reacted with the CaO from the slag, interfering positively in the mechanical properties of the AAC. For the present work it was possible to incorporate up to 28% of RHA.
This addition of RHA in the composition of the AAC influences the CaO/SiO2 ratio, and consequently, the compressive strength. When this ratio is close to 1.0, greater strength results.
With regard to microstructural properties, the formation of CSH is identified in all samples and HT is found in lower CaO/SiO2 ratios (0.49) and for ratios above 1.0 (1.37). In XRD analyses, samples with formation of only one CSH peak and a more amorphous structure develop higher mechanical strengths.
The SiO2/Al2O3 ratio close to 4.5 was not applied in the development of the AAC mixtures in this study. Equal ratios for the two slags showed satisfactory mechanical strength values when applied to AAC_B, but low values when applied to AAC_A (AAC_A = 16 MPa and AAC_B = 40 MPa at 28 days).
With the analyses carried out, the objective of the work of incorporating the RHA to the AAC and verifying its influence on the properties was achieved. Thus, the use of RHA as a component of AAC is suggested when used in conjunction with materials rich in CaO, in order to approximate the CaO/SiO2 ratio of 1.0.
It is worth mentioning that this relationship was tested only for the percentage of 5% sodium hydroxide activator. And tests with other activators should be more thorough.
Furthermore, the relationships used were calculated based on the chemical composition of the precursors, thus it is suggested to consider the degree of amorphism of the material for the development of new studies.
ACKNOWLEDGEMENTS
The authors would like to thank CNPq (National Council for Scientific and Technological Development), process 424896/2018-4, for the financial assistance and Central de Análises of the Federal Technological University of Paraná (UTFPR) by its infrastructure support for the development of this research.
Funding
Data Availability:
How to cite:
REFERENCES
- 1 M. C. G. Juenger, F. Winnefeld, J. L. Provis, and J. H. Ideker, "Advances in alternative cementitious bindesrs," Cement Concr. Res., vol. 41, pp. 1232–1243, 2011.
- 2 E. A. Langaro, C. A. Luz, I. S. Buth, M. C. Moraes, J. I. Pereira Filho, and A. Matoski, "The influence of chemical composition and fineness on the performance of alkali activated cements obtained from blast furnace slags," Matéria (Rio J.), vol. 22, no. 1, pp. e11792, 2017.
- 3 S. Alonso and A. Palomo, "Alkaline activation of metakaolin and calcium hydroxide mixtures: influence of temperature, activator concentration and solids ratio," Mater. Lett., vol. 47, pp. 55–62, 2001.
- 4 C. Shi, A. Fernández-Jiménez, and A. Palomo, "New cements for the 21st century: the pursuit of an alternative to Portland cement," Cement Concr. Res., v. 41, no. 7, pp. 750–763, 2011.
- 5 F. Puertas, M. Palacios, R. Gutiérrez, “Morteros de Escoria Activada Alcalinamente. Propiedades y Durabilidad,” in 2º Congresso Nacional de Argamassas de Construção, 2003.
- 6 M. Ben Haha, B. Lothenbach, and G. Le Saout, "Influence of slag chemistry on the hy-dration of alkali-actived blast-furnace slag - Part I: Effect of MgO," Cement Concr. Res., vol. 41, no. 1, pp. 955–963, 2011.
- 7 M. Ben Haha, B. Lothenbach, and G. Le Saout, "Influence of slag chemistry on the hydra-tion of alkali-actived blast-furnace slag - Part II: Effect of Al2O3," Cement Concr. Res., vol. 42, no. 1, pp. 74–83, 2012.
- 8 A. Nazari, A. Bagheri, and S. Riahi, "Properties of geopolymer with seeded fly ash and rice husk bark ash," Mater. Sci. Eng. A, no. 528, pp. 7395–7401, 2011.
- 9 A. Kusbiantoro, M. F. Nuruddin, N. Shafiq, and S. A. Qaza, "The effect of microwave incinerated rice husk ash on the compressive and bond strength of fly ash based geopolymer concrete," Constr. Build. Mater., no. 36, pp. 695–703, 2012.
- 10 C. Hwang and T. Huynh, "Effect of alkali-activator and rice husk ash content on strength development of fly ash and residual rice husk ash-based geopolymers," Constr. Build. Mater., no. 101, pp. 1–9, 2015.
- 11 P. Sturm, G. J. G. Gluth, H. J. H Brouwers, and H. C. Huhne, "Synthesizing one-part geopolymers from rice husk ash," Constr. Build. Mater., no. 124, pp. 961–966, 2016.
- 12 E. Nimwinya, W. Horpibulsuk, S. Arjharn, T. Phoo-Ngernkham, and A. Poowancum, "A sustainable calcined water treatment sludge and rice husk ash geopolymer," J. Clean. Prod., vol. 119, pp. 128–134, 2016.
- 13 S. O. Sore, A. Messan, E. Prud’homme, G. Escadeillas, and F. Tsobnang, "Synthesis and characterization of geopolymer binders based on local materials from Burkina Faso – Metakaolin and rice husk ash," Constr. Build. Mater., no. 124, pp. 301–311, 2016.
- 14 A. G. N. D. Darsanasiri, F. Matalkah, S. Ramil, K. Aljalode, A. Balachandra, and P. Soroushian, "Ternary alkali aluminosilicate cement based on rice husk ash, slag and coal fly ash," J. Build. Eng., vol. 19, pp. 36–41, Sep. 2018.
- 15 K. D. Shaswat, M. Jyotirmoy, M. M. Syed, A. Adeyemi, R. K. Cyriaque, and D. Debadutta, "Sustainable utilization of ultrafine rice husk ash in alkali activated concrete: characterization and performance evaluation," J. Sustain. Cem.-Based Mater., vol. 11, no. 2, pp. 1–20, 2021.
- 16 S. Chandrasekhar, K. Satyanarayana, P. Pramada, P. Raghavan, and T. Gupta, "Processing, properties and applications of reactive silica from rice husk – an overview," J. Mater. Sci., vol. 32, no. 6, pp. 565–570, 2003.
- 17 M. M. Tashima, L. C. Sousa, J. L. Akasaki, E. J. Silva, J. L. P. Melges, and J. J. P. Bernabeu, "Reuse of rice husk ash in building constructions," HOLOS Environ., vol. 11, no. 1, pp. 81, 2011.
-
18 Instituto Brasileiro de Geografia e Estatística. " Produção de arroz." Brasília: IBGE. https://www.ibge.gov.br/explica/producao-agropecuaria/arroz/br (accessed August 27, 2024).
» https://www.ibge.gov.br/explica/producao-agropecuaria/arroz/br - 19 M. F. M. Zain, M. N. Islam, F. Mahumud, and M. Jamil, "Production of rice husk ash for use in concrete as a supplementary cementitious material," Constr. Build. Mater., vol. 25, no. 2, pp. 798–805, 2011.
- 20 N. Pitt, "Process for preparation of siliceous ashes" U.S. Patent 3959007. 1976.
- 21 J. Hoppe Filho, M. R. Garcez, M. H. F. Medeiros, L. C. P. Silva Filho, and G. C. Isaia, "Reactivity assessment of residual rice-husk ashes," J. Mater. Civ. Eng., vol. 29, no. 6, pp. 2017, Jun 2017.
- 22 L. Hu, Z. He, and S. Zhang, "Sustainable use of rice husk ash in cement-based materials: Environmental evaluation and performance improvement," J. Clean. Prod., vol. 264, pp. 121744, 2020.
- 23 A. Prasara and S. H. Gheewala, "Sustainable utilization of rice husk ash from power plants: a review," J. Clean. Prod., vol. 167, pp. 1020–1028, 2017.
- 24 K. Ganesan, K. Rajagopal, and K. Trangaval, "Rice husk ash blended cement: assessment of optimal level of replacement for strength and permeability properties of concrete," Constr. Build. Mater., vol. 22, pp. 1675–1683, 2008.
- 25 R. Zerbiano, G. Giaccio, and G. C. Isaiaia, "Concrete incorporating rice-husk ash without processing," Constr. Build. Mater., vol. 25, no. 1, pp. 371–378, 2011.
- 26 A. L. G. Gasltadini, G. C. Isaia, A. Saciloto, F. Missau, and T. Hoppe, "Influence of curing time on the chloride penetration resistance of concrete containing rice husk ash: a technical and economical feasibility study," Cement Concr. Compos., vol. 32, pp. 783–793, 2010.
- 27 G. C. Isaia, A. L. G. Gastaldini, T. F. Hoppe, F. Missau, and A. P. Saciloto, "Influence of the use of rice husk ash on the electrical resistivity of concrete: a technical and economic feasibility study," Constr. Build. Mater., vol. 23, pp. 3411–3419, 2009.
- 28 B. S. Thomas, "Green concrete partially comprised of rice husk ash as a supplementary cementitious material – A comprehensive review," Renew. Sustain. Energy Rev., vol. 82, pp. 3913–3923, 2018.
- 29 V. Saraswathy and H. W. Song, "Corrosion performance of rice husk ash blended concrete," Constr. Build. Mater., vol. 21, pp. 1779–1784, 2007.
- 30 D. D. Bui, J. Hu, and P. Stroeven, "Particle size effect on the strength of rice husk ash blended gap-graded Portland cement concrete," Cement Concr. Compos., vol. 27, no. 3, pp. 357–366, 2005.
- 31 M. A. Longhi, E. D. Rodríguez, S. A. Bernal, J. L. Provis, and A. P. Kirchheim, "Valorisation of a kaolin mining waste for the production of geopolymers," J. Clean. Prod., vol. 115, pp. 265–272, 2016.
- 32 D. Salazar-Carreno, R. G. García-Cáceres, and O. O. Ortíz-Rodríguez, "Laboratory processing of Colombian rice husk for obtaining amorphous silica as concrete supplementary cementing material," Constr. Build. Mater., vol. 96, pp. 65–75, 2015.
- 33 S. C. Pal, A. Mukherjee, and S. R. Pathak, "investigation of hydraulic activity of ground granuleted blast furnace slag in concrete," Cement Concr. Res., vol. 33, no. 9, pp. 1481–1486, 2003.
- 34 E. A. Langaro, C. A. da Luz, I. S. Buth, M. C. Moraes, J. I. Pereira Filho, and A. Matoski, "The influence of chemical composition and fineness on the performance of alkali activated cements obtained from blast furnace slags," Matéria (Rio J.), vol. 22, no. 1, pp. e11792, 2017.
- 35 W. Chen and H. J. H. Brouwers, "The hydration of slag, part 1: reaction models for alkali-activated slag," J. Mater. Sci., vol. 42, no. 2, pp. 428–443, 2007.
- 36 A. Gruskovnjak, B. Lothenbach, L. Holzer, R. Figi, and F. Winnefeld, "Hydration of alkali-activated slag: comparison with ordinary Portland cement," Adv. Cem. Res., vol. 18, no. 3, pp. 119–128, 2006.
- 37 H. F. W. Taylor, Cement Chemestry, Cambridge, MA, USA: Academic Press, 1997.
- 38 J. Pérez-Ramírez, and S. Abelló, "Thermal decomposition of hydrotalcite-like compounds studied by a novel tapered element oscillating microbalance (TEOM): comparison with TGA and DTA," Thermochim. Acta, vol. 444, no. 1, pp. 75–82, 2006.
- 39 G. Ya-Min, F. Yong-hao, Y. Duo, G. Yong-fan, and Z. Chen-hui, "Properties and microstructure of alkali-activated slag cement cured at below- and about-normal temperature," Constr. Build. Mater., vol. 79, pp. 1–8, 2015.
- 40 A. Font et al., "Design and properties of 100% waste-based ternary alkali-activated mortars: Blast furnace slag, olive-stone biomass ash and rice husk ash," J. Clean. Prod., vol. 243, pp. 118568, Jan. 2020.