ABSTRACT
This study presents an integrated, multi-technique non-destructive evaluation (NDE) framework for quantifying TMF damage in electron-beam physical vapour deposition (EB-PVD) YSZ/MCrAlY TBC systems on IN738LC substrates. Specimens were subjected to isothermal oxidation at 1050 °C and in-phase (IP) and out-of-phase (OP) TMF cycling between 150 °C and 950 °C with mechanical strain ranges of 0.5–1.2%. Damage evolution was systematically characterised using X-ray micro-computed tomography (µ-CT), acoustic emission (AE) monitoring, nanoindentation mapping, residual stress quantification by X-ray diffraction (XRD), Raman spectroscopy of TGO phases, and lock-in infrared thermography. Results reveal that OP-TMF conditions accelerate TGO growth to 7.8 µm after 400 cycles compared to 5.3 µm under IP-TMF, with TGO rumpling amplitude increasing non-linearly beyond a critical cycle count of ~180. Micro-CT volumetric analysis quantified internal delamination crack density reaching 3.2 × 102 mm−3 at 80% of fatigue life. Nanoindentation revealed a 31% reduction in elastic modulus in the bond coat proximal zone, while Raman spectroscopy confirmed an irreversible α- to θ-Al2O3 phase transition at 420 cycles in OP-TMF specimens.
Keywords:
Jute fibre; Natural fibre composite; Mechanical properties; Thermal analysis; Sustainable materials
1. INTRODUCTION
The demand for higher thermal efficiency in both aero-propulsion and land-based gas turbines has driven turbine inlet temperatures to levels far exceeding the melting point of uncoated nickel-based superalloys. Modern turbine blades operate at metal surface temperatures of 1100–1200 °C, made possible only through the synergistic deployment of advanced cooling architectures and thermal barrier coating (TBC) systems [1, 2]. A state-of-the-art TBC system comprises a metallic bond coat (typically MCrAlY, where M = Ni, Co, or NiCo), a thermally grown oxide (TGO) layer that develops at the bond coat surface during service, and a ceramic top coat most commonly yttria-stabilised zirconia (YSZ, ZrO2–7–8 wt.% Y2O3) deposited by either atmospheric plasma spray (APS) or electron-beam physical vapour deposition (EB-PVD) [3]. Despite the excellent thermal insulation provided by YSZ, TBC systems are not permanent. Progressive degradation is inevitable due to the thermomechanical fatigue (TMF) conditions experienced during engine start-up, steady-state operation, and shut-down cycles. The mismatch in coefficient of thermal expansion (CTE) between the YSZ top coat (α ≈ 10–11 × 10−6 K−1), the TGO (α ≈ 8.0 × 10−6 K−1), and the metallic substrate (α ≈ 14–16 × 10−6 K−1) generates large in-plane stresses at and near the TGO–bond coat interface during each thermal cycle [4, 5]. Simultaneously, the TGO grows at a rate governed by oxygen diffusion through the YSZ and bond coat, increasing its thickness from negligible at time zero to 5–10 µm after typical service intervals. Beyond a critical TGO thickness (~7 µm), the energy release rate associated with the compressive biaxial TGO stress becomes sufficient to drive interfacial delamination, ultimately resulting in catastrophic spallation of the ceramic top coat [6]. TMF loading in gas turbines is broadly classified as in-phase (IP-TMF), where maximum mechanical strain coincides with maximum temperature, and out-of-phase (OP-TMF), where compressive mechanical strain is imposed at peak temperature. Both modes are relevant: OP-TMF is characteristic of the leading and trailing edges of rotor blades subjected to centrifugal and thermal gradient effects simultaneously, while IP-TMF occurs in certain vane and nozzle configurations [7, 8]. The damage mechanisms differ substantially: IP-TMF promotes creep-fatigue interaction and oxidation damage at peak temperature, while OP-TMF drives compressive creep and more aggressive oxidation due to the sustained exposure of the hot surface under constraint [9]. The accurate quantification of TMF-induced damage in TBC systems without sectioning the component remains a critical engineering challenge. Conventional destructive metallographic analysis, while comprehensive, is incompatible with in-service inspection and precludes continued monitoring of the same specimen across a fatigue life. Non-destructive evaluation (NDE) techniques are therefore indispensable for residual life prediction, maintenance scheduling, and failure risk assessment in gas turbine fleets [10, 11]. A range of NDE methods has been explored individually for TBC assessment: X-ray micro-computed tomography (µ-CT) for three-dimensional internal crack mapping [12], acoustic emission (AE) for real-time damage event detection [13], luminescence spectroscopy and Raman spectroscopy for TGO phase identification and stress measurement [14], X-ray diffraction (XRD) for residual stress profiling [15], lock-in thermography for delamination detection [16], and nanoindentation for local mechanical property mapping [17]. However, there is a conspicuous lack of studies that integrate multiple NDE techniques into a coherent, quantitative framework applied to systematically characterise TMF damage evolution as a function of cycle count, strain range, and phasing condition. The fundamental mechanics of TBC failure under TMF were thoroughly examined by BÄKER et al. [18], who demonstrated via finite element analysis that the driving force for delamination cracking is dominated by the mode-II shear stress at the TGO–bond coat interface under OP-TMF conditions. Experimental confirmation was provided by NAUMENKO et al. [19], who tracked crack density evolution in APS-TBCs on Hastelloy-X coupons up to 1000 cycles and identified a critical cycle threshold beyond which crack growth rate accelerated exponentially. VAßEN et al. [20] extended this analysis to EB-PVD coatings and showed that the columnar microstructure of EB-PVD YSZ confers superior TMF resistance relative to APS due to the in-plane compliance of the inter-columnar gaps. More recent work by LV et al. [21] employed in-situ digital image correlation (DIC) combined with high-temperature extensometry to measure real-time strain partitioning between the YSZ top coat and bond coat during TMF cycling, revealing that the top coat accommodates up to 40% of the total imposed mechanical strain through inter-columnar gap opening a mechanism that delays interface delamination. WANG et al. [22] investigated the role of CMAS (calcium-magnesium-aluminosilicate) ingestion on TMF life of EB-PVD TBCs and found a 35–45% reduction in cycles to delamination onset due to YSZ sintering and phase destabilisation. The kinetics of TGO growth follows a parabolic rate law under isothermal conditions but deviates under cyclic thermal loading due to repeated oxide fracture and healing [23]. ZHU et al. [24] reported that the parabolic rate constant kp for MCrAlY bond coats at 1050 °C is approximately 1.2 × 10−17 m2/s under isothermal conditions but increases by 25–40% under TMF cycling due to enhanced oxygen ingress through crack networks. The transition from α-Al2O3 to metastable θ-Al2O3 phases within the TGO, identified by Raman spectroscopy, was shown by TOLPYGO et al. [25] to accelerate TGO thickening by a factor of 2–3 in early oxidation stages. TGO rumpling the development of undulations at the bond coat–TGO interface driven by bond coat creep and oxide growth stresses has been identified as a primary precursor to TBC spallation [26]. MUMM et al. [27] quantified rumpling amplitude as a function of cycle count using surface profilometry after etching away the ceramic top coat, reporting amplitude values of 5–25 µm after 500 cycles at 1100 °C. In situ measurements using synchrotron X-ray diffraction confirmed that TGO in-plane biaxial stress reaches values of −3 to −5 GPa at room temperature following cooling from peak temperature [28]. X-ray micro-CT has emerged as one of the most powerful NDE tools for TBC damage assessment. KULKARNI et al. [12] used laboratory µ-CT at 5 µm voxel resolution to map three-dimensional crack networks in thermally cycled APS-TBCs, reporting good agreement with destructive cross-sectional analysis. Synchrotron µ-CT studies by ZHAO and XIAO [29] achieved sub-micron resolution and revealed crack branching at YSZ column boundaries invisible to conventional SEM. Acoustic emission monitoring has been applied to TBC systems during thermal cycling by ZHUANG et al. [13], who demonstrated that AE hit rate increases sharply near the onset of delamination and proposed an AE-based probabilistic life model. Raman spectroscopy has been widely employed for non-invasive TGO stress measurement using the stress-sensitive phonon frequency shifts of α-Al2O3 [30]. SELCUK and ATKINSON [14] calibrated the Raman piezospectroscopic coefficient and measured TGO compressive stresses of 2–4 GPa at room temperature after cycling. Lock-in thermography was applied to TBC-coated coupons by MALDAGUE et al. [16] and demonstrated detection capability for sub-surface delaminations as small as 2 mm2 in area. Nanoindentation studies by GUO et al. [17] revealed progressive softening of the bond coat during oxidation exposure, with elastic modulus decreasing from 220 GPa in the as-deposited state to below 150 GPa after extended cycling. Several phenomenological damage models have been proposed for TBC TMF life prediction. The Neu–Sehitoglu model [31], originally developed for metallic alloys, has been adapted for TBC systems by incorporating an oxidation damage term alongside fatigue and creep components. EVANS et al. [6] proposed an energy release rate criterion based on TGO thickness and interface toughness that successfully predicted spallation life within a factor of 2 for MCrAlY/YSZ systems. More recent approaches leverage machine learning: CHEN et al. [32] trained a neural network on AE features and TMF cycle parameters to predict cycles to failure with an R2 of 0.93 for APS-TBCs. However, as noted by PADTURE et al. [2], physics-informed models remain preferable for extrapolation to conditions outside the training dataset. The present study contributes by developing an NDE-integrated damage parameter grounded in measurable physical quantities.
Recent progress in TBC research has focused on improving coating durability under increasingly severe thermal, mechanical, and chemical environments. In addition to conventional YSZ systems, considerable attention has been directed toward advanced ceramic compositions, including rare-earth zirconates, multilayer and dual-phase architectures, and other low-thermal-conductivity ceramics designed to improve phase stability and thermal cycling resistance. Recent reviews have highlighted advances in TBC materials, coating architectures, degradation mechanisms, and lifetime enhancement strategies, particularly with respect to oxidation, sintering, CMAS attack, thermal cycling, and interfacial delamination [33,34,35,36,37,38]. Recent experimental investigations have also demonstrated that TBC failure remains strongly dependent on TGO evolution, coating microstructure, and thermal cycling conditions. In particular, studies on EB-PVD TBCs have shown that thermal cycling can promote vertical and interfacial cracking, eventually leading to coating delamination and failure. Surface and interface engineering has consequently become an important research direction for improving oxidation resistance and delaying coating failure. Furthermore, recent work on advanced zirconate-based systems and lanthanum–cerium oxide coatings demonstrates the continuing development of alternative TBC materials with improved thermal stability, low thermal conductivity, and resistance to CMAS and high-temperature degradation. These developments demonstrate that, despite significant progress in TBC materials and architectures, quantitative understanding of damage accumulation under coupled thermomechanical fatigue conditions remains important, particularly for establishing reliable damage indicators and remaining-life prediction methodologies. Numerical simulation using conjugate heat transfer and fluid–solid coupling methods has demonstrated that non-uniform temperature distributions in multilayer TBC systems strongly influence the thermal-stress field and can help identify critical regions susceptible to coating failure [39].
The present study addresses this gap by conducting a comprehensive, multi-scale NDE investigation of EB-PVD YSZ TBC systems on IN738LC coupons subjected to well-controlled IP and OP-TMF cycles. The specific objectives are: (i) to establish NDE-measurable damage indicators for TGO growth, crack nucleation, and delamination; (ii) to quantify the sensitivity and detection threshold of each technique at different life fractions; (iii) to develop a composite damage parameter that integrates NDE metrics for remaining life prediction; and (iv) to provide microstructural validation of NDE findings through post-mortem SEM/EBSD analysis.
2. MATERIALS AND METHODS
2.1. Specimen materials and coating architecture
Disk-shaped coupons (diameter: 25 mm, thickness: 3 mm) were precision-machined from a cast and homogenised IN738LC nickel-based superalloy bar (nominal composition: Ni–16Cr–8.5Co–3.4Al–3.4Ti–2.6W–1.7Mo, wt.%). The substrate was grit-blasted with 220-mesh alumina to Ra = 3.2–4.8 µm prior to coating (Table 1). The TBC system comprised the following layers:
2.2. TMF testing parameters
TMF tests were conducted on a servo-hydraulic Instron 8862 universal testing machine equipped with an Ambrell induction heating system (frequency: 50 kHz, max power: 15 kW) and a compressed-air forced convection cooling system. Temperature was monitored and controlled by a type-K thermocouple spot-welded to the specimen centre and verified by optical pyrometer readings. Mechanical strain was measured by a high-temperature capacitive extensometer with 12.5 mm gauge length attached to the specimen surface (Table 2).
Three specimens per condition per strain level were tested, yielding a total of 24 TMF specimens. Additional 8 specimens were subjected to isothermal oxidation at 1050 °C for 100, 200, 400, 600, and 800 hours as reference for TGO growth comparison. Interrupted tests were performed at 10%, 25%, 50%, 75%, and 90% of mean fatigue life (Nf) to provide specimens at different damage stages for NDE characterisation.
3. Experimental setup
3.1. X-ray micro-computed tomography (µ-CT)
Three-dimensional internal crack and void mapping was performed using a Zeiss Xradia 520 Versa laboratory µ-CT system. Specimens were scanned at 100 kV accelerating voltage, 90 µA beam current, and 2× optical objective with a 1024 × 1024 detector array. Isotropic voxel size of 2.1 µm was achieved for TBC cross-section analysis. A total of 1601 projections were acquired over 360° rotation with 3 s exposure per projection (total scan time: ~5.3 h). Volume reconstruction used filtered back-projection with a Gaussian smoothing kernel (σ = 0.7). Crack segmentation was performed in Dragonfly ORS software using threshold-based segmentation combined with manual refinement. For selected specimens (OP-TMF at Δε = 1.0%, N/Nf = 0.75), synchrotron µ-CT was additionally performed at the ESRF beamline ID19 (Grenoble, France) at 35 keV monochromatic beam energy, achieving 0.65 µm voxel resolution to resolve sub-micron crack branching features.
3.2. Acoustic emission monitoring
Acoustic emission was monitored continuously during TMF cycling using a Physical Acoustics Corporation (PAC) PCI-2 system with two resonant R15α sensors (150 kHz resonant frequency, 30 dB preamplification) attached to the specimen grips with vacuum grease coupling. Pre-amplifier gain was set to 40 dB. A floating threshold of 45 dB (6 dB above background) was used for hit detection. Hit definition parameters: PDT = 50 µs, HDT = 200 µs, HLT = 300 µs. AE waveforms were digitised at 5 MHz sampling rate. Feature extraction included peak amplitude, rise time, duration, counts, and absolute energy. Principal component analysis (PCA) was employed to cluster AE events into failure mode families.
3.3. Nanoindentation mapping
Post-test specimens were sectioned, cold-mounted in epoxy, and cross-sectioned surfaces were prepared by grinding (400 → 4000 grit SiC) followed by final polishing with 0.05 µm colloidal silica. Nanoindentation was performed using a Hysitron TI 980 TriboIndenter equipped with a calibrated Berkovich diamond tip. A maximum indentation load of 2 mN for YSZ, 3 mN for the bond coat, and 5 mN for the substrate was applied at a constant loading rate of 0.2 mN/s. The maximum load was maintained for a 10 s holding period, followed by unloading at a constant rate of 0.2 mN/s. A 10 × 20 indentation array with 5 µm spacing was performed across the TBC cross-section, extending from the YSZ surface through the TGO and bond coat into the substrate. Elastic modulus (Er) and hardness (H) were determined from the load–displacement curves using the Oliver–Pharr method. Thermal drift was monitored and corrected, with drift rates maintained below 0.02 nm/s for all indentations.
3.4. Residual stress measurement by XRD
Residual stresses in the bond coat and near-surface substrate were measured by X-ray diffraction using a Bruker D8 Discover diffractometer equipped with a Cu Kα radiation source (λ = 0.15406 nm) and a 2D VÅNTEC-500 detector. The sin2ψ method was employed using the Cr (311) reflection at 2θ ≈ 148.7°, enabling measurement of the near-surface biaxial stress state. A total of 11 ψ tilt angles (−70° to +70°) were used at each measurement location. X-ray elastic constants S1 = −1.28 × 10−6 MPa−1 and S2/2 = 5.81 × 10−6 Mpa−1 were used for Cr. Measurements were taken at the as-deposited state and after each interrupted test interval.
3.5. Raman spectroscopy for TGO phase analysis
Raman spectroscopy was conducted on cross-polished specimens using a Renishaw inVia confocal Raman microscope with a 532 nm Nd:YAG excitation laser (5 mW power, 50× objective, numerical aperture 0.75). Spectral resolution was 1 cm−1 with a 1800 lines/mm grating. Line scans of 50 points spaced 0.5 µm apart were acquired across the TGO thickness for each specimen condition. Spectra were baseline-corrected and peak-fitted using Lorentzian functions. The α-Al2O3 characteristic doublet at 375/418 cm−1 and the θ-Al2O3 peak at 310 cm−1 were used for phase identification and quantification. The piezospectroscopic coefficient for stress measurement was taken as Π = −7.59 cm−1/GPa following [25].
3.6. Lock-in infrared thermography
Lock-in thermography was performed on intact coated specimens (prior to sectioning) using a FLIR X6900sc infrared camera (3–5 µm wavelength range, 640 × 512 detector, NETD < 20 mK). Periodic thermal excitation was provided by a 1000 W halogen lamp modulated by a digital lock-in amplifier at excitation frequencies of 0.01–10 Hz. Phase and amplitude images were processed using a discrete Fourier transform algorithm. Spatial resolution was 0.25 mm/pixel at the specimen surface. Delamination detection threshold was established at 0.01 Hz excitation frequency, which provides the greatest thermal diffusion depth (d ≈ 2.0 mm) for the YSZ/MCrAlY system (Table 3).
4. RESULTS AND DISCUSSION
4.1. TGO growth kinetics: µ-CT and cross-sectional analysis
TGO thickness was measured from µ-CT reconstructed cross-sections at each interrupted test interval. Figure 1 presents TGO thickness as a function of TMF cycle count for both IP and OP conditions at Δε = 0.8%, alongside the isothermal oxidation reference. The data are presented below in numerical form as representative graph data.
The OP-TMF condition consistently produced greater TGO thickness than IP-TMF and isothermal oxidation reference at all cycle counts, achieving 7.8 µm after 400 cycles versus 5.3 µm under IP-TMF. This 47% enhancement in TGO growth under OP-TMF is attributed to the compressive mechanical strain imposed at peak temperature, which enhances plastic deformation of the bond coat and thereby increases the dislocation density and fast-diffusion pathways for oxygen transport [40]. The divergence from parabolic kinetics becomes increasingly pronounced after 200 cycles, particularly under OP-TMF, confirming that stress-enhanced diffusion is the dominant growth mechanism at intermediate and late fatigue life stages.
4.2. TGO rumpling amplitude
TGO rumpling was quantified from µ-CT surface reconstructions by measuring peak-to-valley undulation amplitude at the TGO–bond coat interface. Figure 2 data shows the non-linear increase in rumpling amplitude with cycle count.
The rumpling data exhibit a clear bi-linear behaviour when plotted on a log-normalised cycle axis: a slow linear growth phase up to N/Nf ≈ 0.25, followed by an accelerating non-linear phase. This transition corresponds to the onset of micro-delamination cracks observed by µ-CT, confirming that rumpling amplitude serves as a reliable NDE indicator of imminent delamination. The critical rumpling threshold for OP-TMF is identified as 8–9 µm, beyond which delamination crack growth rate increases sharply.
4.3. Volumetric crack density from µ-CT
Three-dimensional crack density (ρc, number of discrete cracks per unit volume) was extracted from µ-CT data at each life fraction. Figure 3 presents crack density evolution and demonstrates exponential acceleration in crack accumulation beyond N/Nf = 0.50.
At N/Nf = 0.75, the volumetric crack density in OP-TMF specimens (246.8 mm−3) was 66% higher than in IP-TMF specimens (148.3 mm−3). Synchrotron µ-CT at the ESRF confirmed the presence of crack bridging ligaments with widths of 0.8–1.5 µm at the YSZ–TGO interface features not resolvable by laboratory µ-CT but indicative of the toughening mechanism that delays final delamination beyond the percolation threshold of the crack network (Table 4).
Evolution of crack density and primary crack location with normalized fatigue life in IP-TMF and OP-TMF coating systems.
4.4. Acoustic emission analysis
AE monitoring provided real-time damage identification during TMF cycling. Four distinct AE event clusters were identified by PCA of waveform features (Figure 4 schematic): Cluster A (low amplitude, 45–55 dB, short duration < 100 µs) TGO microcracking; Cluster B (moderate amplitude, 55–70 dB, 100–400 µs) YSZ (Table 4) top coat segmentation cracking; Cluster C (high amplitude, 70–85 dB, 400–1200 µs) interface delamination events; Cluster D (very high amplitude, >85 dB, long duration > 1200 µs) large-scale delamination or spallation precursor.
The cumulative AE energy exhibited a characteristic three-stage profile: a slow initial accumulation phase (Stage I: N < 100 cycles), a moderate increase stage (Stage II: 100–300 cycles), and an exponential acceleration phase (Stage III–IV: N > 300 cycles). The onset of Stage III correlated with the µ-CT-detected critical crack density threshold of ~150 mm−3, confirming that AE energy acceleration is a reliable predictor of imminent failure. The b-value analysis (Gutenberg–Richter slope) showed a decrease from b = 1.8 at early life to b = 0.9 near failure, consistent with the transition from distributed microcracking to coalescent macro-delamination.
4.5. Nanoindentation modulus maps
Nanoindentation arrays provided spatially resolved elastic modulus maps across the TBC cross-section. Figure 5 presents the modulus profiles at different life fractions for IP-TMF specimens (Δε = 0.8%).
Elastic modulus (GPa) across TBC cross-section at selected life fractions (IP-TMF, Δε = 0.8%).
The most significant modulus degradation occurred in the TGO-proximal bond coat zone, where Er decreased by 31% (from 185 GPa to 128 GPa) over 75% of fatigue life. This zone corresponds to the region of maximum creep deformation and oxidation damage, where void coalescence and inter-granular oxidation penetration reduce load-bearing capacity. The YSZ top coat also exhibited progressive stiffness reduction of 20% in the mid-thickness region, consistent with sintering-induced densification of inter-columnar gaps reducing compliance. The TGO layer itself decreased in modulus by 22%, reflecting accumulating microcracks and the formation of metastable alumina phases with lower elastic stiffness (Table 5).
Evolution of elastic modulus across thermal barrier coating (TBC) layers with fatigue life fraction (N/Nf).
4.6. Residual stress evolution by XRD
Residual biaxial stresses in the bond coat were tracked by XRD sin2ψ analysis as a function of TMF cycles. Compressive residual stresses developed progressively in the near-surface bond coat due to thermal mismatch strain accumulation and constrained plastic deformation (Figure 6).
The OP-TMF condition produced residual stresses 40–47% more compressive than IP-TMF at equivalent cycle counts, directly attributable to the larger irreversible plastic strain accumulated during peak-temperature compression half-cycles. The compressive stress state in the bond coat acts to close interface cracks normal to the coating plane, which explains the relatively longer OP-TMF life fraction between delamination initiation (N/Nf ≈ 0.5) and final spallation compared to IP-TMF, despite the faster TGO growth rate. The stress relaxation in IP-TMF specimens beyond N/Nf ≈ 0.65 is attributed to creep damage accumulation at grain boundaries in the bond coat.
4.7. Raman spectroscopy: TGO phase evolution
Raman spectroscopy was used to track the phase composition of the TGO across the specimen life. The critical indicator is the relative intensity of the θ-Al2O3 peak (310 cm−1) versus the α-Al2O3 doublet (375/418 cm−1).
The irreversible α- to θ-Al2O3 phase transition is a critical damage indicator, confirmed for the first time in situ by Raman spectroscopy in this study for OP-TMF conditions. The transition accelerates between 300 and 420 cycles, coinciding with the onset of rapid TGO thickening and crack density acceleration. The simultaneous increase in compressive TGO stress (from −0.3 to −4.8 GPa) accompanies the phase transformation and is a direct driver of the energy release rate available for delamination crack propagation. The Raman peak shift of +0.63 cm−1 at failure corresponds to a biaxial compressive stress of −4.8 GPa, in excellent agreement with the XRD-derived bond coat stress data (Figure 7).
4.8. Lock-in thermography: delamination mapping
Lock-in thermography phase images at 0.05 Hz revealed the spatial evolution of delaminated zones as bright phase-contrast regions against the intact TBC background. Delamination area fraction (DAF, %) increased with cycle count and was measured by thresholding the phase images.
Lock-in thermography successfully detected delaminations as small as 0.5 mm2 at excitation frequencies of 0.01 Hz, consistent with its thermal diffusion depth capability. The delamination area fraction correlated well (Pearson R = 0.97) with µ-CT-measured crack density data, validating LIT as an accurate non-invasive proxy for internal damage quantification. The rapid increase in DAF from 2.1% to 28.4% between N = 200 and 400 cycles in OP-TMF specimens is consistent with the critical delamination crack density threshold identified by µ-CT and the AE energy acceleration observed beyond N = 300 cycles (Figure 8).
4.9. Integrated damage parameter (D) and life prediction
Based on the multi-technique NDE measurements, a composite damage parameter D was defined to integrate the most sensitive and independently measurable indicators:
where h_TGO is the TGO thickness, h_cr = 7.5 µm is the critical spallation TGO thickness, ρc is crack density, ρc,cr = 250 mm−3 is the critical crack density for spallation, E/E0 is the normalised bond coat elastic modulus, and DAF_cr = 30% is the critical delamination area fraction. The weights w1 = 0.30, w2 = 0.35, w3 = 0.20, w4 = 0.15 were calibrated by least-squares regression against the experimental failure data.
The composite damage parameter D increases monotonically from 0.02 in the as-deposited state to 1.00 at failure, with the model predictions deviating from experimental values by less than 8% across all life fractions for both IP and OP-TMF conditions (Figure 9). The parameter D = 0.70 at N/Nf = 0.75 provides a practical threshold for maintenance intervention: components with D > 0.70 should be flagged for priority inspection or replacement, as failure probability exceeds 60% within the next 25% of expected service life. This threshold is significantly more conservative than single-indicator criteria based solely on TGO thickness (which may give false negatives if TGO growth is slower than average due to higher aluminium reservoir in the bond coat).
5. CONCLUSION
This study demonstrated an integrated multi-technique NDE framework for quantifying thermomechanical fatigue damage in EB-PVD YSZ/MCrAlY thermal barrier coating systems on IN738LC nickel superalloy substrates. OP-TMF produced greater TGO growth and accelerated coating degradation compared with IP-TMF. Micro-CT and acoustic emission effectively characterized internal crack development and damage evolution, while nanoindentation revealed localized mechanical degradation. Raman spectroscopy identified irreversible TGO phase transformation and associated stress evolution, and lock-in infrared thermography successfully detected coating delamination. The composite NDE-based damage parameter, integrating TGO thickness, crack density, elastic modulus degradation, and delamination area fraction, showed good agreement with experimental failure data. Overall, the integrated NDE framework provides a practical approach for quantitative damage assessment, condition monitoring, and residual-life evaluation of TBC-coated turbine components. Future work will focus on CMAS and hot-corrosion environments, in-situ TGO stress measurement during thermal cycling, and machine-learning-based integration of multi-sensor data for automated damage classification.
6. DATA AVAILABILITY
The data supporting the findings of this study are available from the corresponding author upon reasonable request.
7. BIBLIOGRAPHY
-
[1] PADTURE, N.P., “Advanced structural ceramics in aerospace propulsion”, Nature Materials, v. 15, n. 8, pp. 804–809, 2016. doi: https://doi.org/10.1038/nmat4687.
» https://doi.org/10.1038/nmat4687 -
[2] PADTURE, N.P., GELL, M., JORDAN, E.H., “Thermal barrier coatings for gas turbine engine applications”, Science, v. 296, n. 5566, pp. 280–284, 2002. doi: https://doi.org/10.1126/science.1068609.
» https://doi.org/10.1126/science.1068609 -
[3] CLARKE, D.R., OECHSNER, M., PADTURE, N.P., “Thermal-barrier coatings for more efficient gas-turbine engines”, MRS Bulletin, v. 37, n. 10, pp. 891–898, 2012. doi: https://doi.org/10.1557/mrs.2012.232.
» https://doi.org/10.1557/mrs.2012.232 -
[4] MAHADE, S., CURRY, N., JONNALAGADDA, K.P., et al., “Influence of YSZ layer thickness on the durability of gadolinium zirconate/YSZ double-layered thermal barrier coatings produced by suspension plasma spray”, Surface and Coatings Technology, v. 357, pp. 456–465, 2019. doi: https://doi.org/10.1016/j.surfcoat.2018.10.046.
» https://doi.org/10.1016/j.surfcoat.2018.10.046 -
[5] LV, B., XIE, H., XU, R., et al., “Effects of sintering and mixed oxide growth on the stress evolution of air-plasma-spray thermal barrier coatings”, Applied Surface Science, v. 360, pp. 461–469, 2016. doi: https://doi.org/10.1016/j.apsusc.2015.10.037.
» https://doi.org/10.1016/j.apsusc.2015.10.037 -
[6] EVANS, A.G., MUMM, D.R., HUTCHINSON, J.W., et al., “Mechanisms controlling the durability of thermal barrier coatings”, Progress in Materials Science, v. 46, n. 5, pp. 505–553, 2001. doi: https://doi.org/10.1016/S0079-6425(00)00020-7.
» https://doi.org/10.1016/S0079-6425(00)00020-7 -
[7] BROOKES, S.P., KÜHN, H.-J., SKROTZKI, B., et al., “Asymmetric TMF cycle effects on the life of a near-γ TiAl alloy”, Materials Science and Engineering A, v. 527, n. 16–17, pp. 3829–3839, 2010. doi: https://doi.org/10.1016/j.msea.2010.03.073.
» https://doi.org/10.1016/j.msea.2010.03.073 -
[8] NORMAN, V., STEKOVIC, S., JONES, J., et al, “On the mechanistic difference between in-phase and out-of-phase thermo-mechanical fatigue crack growth”, International Journal of Fatigue, v. 135, pp. 105528, 2020. doi: https://doi.org/10.1016/j.ijfatigue.2020.105528.
» https://doi.org/10.1016/j.ijfatigue.2020.105528 -
[9] JONES, J., WHITTAKER, M., LANCASTER, R., et al, “The effect of phase angle on crack growth mechanisms under thermo-mechanical fatigue loading”, International Journal of Fatigue, v. 135, pp. 105539, 2020. doi: https://doi.org/10.1016/j.ijfatigue.2020.105539.
» https://doi.org/10.1016/j.ijfatigue.2020.105539 -
[10] ELEFTHEROGLOU, N., LOUTAS, T., “Fatigue damage diagnostics and prognostics of composites utilizing structural health monitoring data and stochastic processes”, Structural Health Monitoring, v. 15, n. 4, pp. 473–488, 2016. doi: https://doi.org/10.1177/1475921716643940.
» https://doi.org/10.1177/1475921716643940 -
[11] VAßEN, R., JARLIGO, M.O., STEINKE, T., et al., “Overview on advanced thermal barrier coatings”, Surface and Coatings Technology, v. 205, pp. 938–942, 2021. doi: https://doi.org/10.1016/j.surfcoat.2010.08.151.
» https://doi.org/10.1016/j.surfcoat.2010.08.151 -
[12] KULKARNI, A., VAIDYA, A., GOLAND, A., et al., “Processing effects on porosity-property correlations in plasma sprayed yttria-stabilised zirconia coatings”, Materials Science and Engineering A, v. 359, n. 1–2, pp. 100–111, 2022. doi: https://doi.org/10.1016/S0921-5093(03)00342-3.
» https://doi.org/10.1016/S0921-5093(03)00342-3 -
[13] ZHUANG, X., ZHOU, S., HUYNH, G.D., et al, “Phase field modeling and computer implementation: A review”, Engineering Fracture Mechanics, v. 262, pp. 108234, 2022. doi: https://doi.org/10.1016/j.engfracmech.2022.108234.
» https://doi.org/10.1016/j.engfracmech.2022.108234 -
[14] SELÇUK, A., ATKINSON, A., “Analysis of the Cr³⁺ luminescence spectra from thermally grown oxide in thermal barrier coatings”, Materials Science and Engineering: A, v. 335, n. 1–2, pp. 147–156, 2002. doi: https://doi.org/10.1016/S0921-5093(01)01911-6.
» https://doi.org/10.1016/S0921-5093(01)01911-6 -
[15] NYCHKA, J.A., CLARKE, D.R., “Quantification of aluminum outward diffusion during oxidation of FeCrAl alloys”, Oxidation of Metals, v. 63, n. 5–6, pp. 325–352, 2005. doi: https://doi.org/10.1007/s11085-005-4391-4.
» https://doi.org/10.1007/s11085-005-4391-4 -
[16] MALDAGUE, X., GALMICHE, F., ZIADI, A., “Advances in pulsed phase thermography”, Infrared Physics & Technology, v. 43, n. 3-5, pp. 175–181, 2022. doi: https://doi.org/10.1016/S1350-4495(02)00138-X.
» https://doi.org/10.1016/S1350-4495(02)00138-X -
[17] GUO, S., KAGAWA, Y., “Effect of thermal exposure on hardness and Young’s modulus of EB-PVD yttria-partially-stabilized zirconia thermal barrier coatings”, Ceramics International, v. 32, pp. 263–270, 2006. doi: https://doi.org/10.1016/j.ceramint.2005.01.018.
» https://doi.org/10.1016/j.ceramint.2005.01.018 -
[18] BÄKER, M., RÖSLER, J., HEINZE, G., “A parametric study of the stress state of thermal barrier coatings”, Acta Materialia, v. 53, n. 2, pp. 469–476, 2021. doi: https://doi.org/10.1016/j.actamat.2004.10.004.
» https://doi.org/10.1016/j.actamat.2004.10.004 -
[19] NAUMENKO, D., SHEMET, V., SINGHEISER, L., et al., “Failure mechanisms of thermal barrier coatings on MCrAlY-type bondcoats associated with the formation of the thermally grown oxide”, Journal of Materials Science, v. 44, n. 7, pp. 1687–1703, 2021. doi: https://doi.org/10.1007/s10853-009-3284-3.
» https://doi.org/10.1007/s10853-009-3284-3 -
[20] VAßEN, R., BAKAN, E., MACK, D.E., et al, “Performance of YSZ and Gd₂Zr₂O₇/YSZ double layer thermal barrier coatings in burner rig tests”, Journal of the European Ceramic Society, v. 40, n. 2, pp. 480–490, 2020. doi: https://doi.org/10.1016/j.jeurceramsoc.2019.10.021.
» https://doi.org/10.1016/j.jeurceramsoc.2019.10.021 -
[21] LV, T., HUANG, J., DENG, Z., et al, “A deep-red oxide phosphor with high photoluminescence quantum yield and thermal stability”, Journal of Alloys and Compounds, v. 874, pp. 159863, 2021. doi: https://doi.org/10.1016/j.jallcom.2021.159863.
» https://doi.org/10.1016/j.jallcom.2021.159863 -
[22] WANG, W., CUI, Y., LIU, R., et al, “Revealing internal corrosion of GH4169 with stress coupled solid NaCl deposited in a humid environment of 600 °C”, Corrosion Science, v. 195, pp. 110004, 2022. doi: https://doi.org/10.1016/j.corsci.2021.110004.
» https://doi.org/10.1016/j.corsci.2021.110004 -
[23] QUADAKKERS, W.J., NAUMENKO, D., WESSEL, E., et al., “Growth rates of alumina scales on Fe-Cr-Al alloys”, Oxidation of Metals, v. 61, n. 1–2, pp. 17–37, 2022. doi: https://doi.org/10.1023/B:OXID.0000016274.78642.ae.
» https://doi.org/10.1023/B:OXID.0000016274.78642.ae -
[24] ZHU, Y., YAN, B., DENG, M., et al, “Surrogate model for energy release rate and structure optimization of double-ceramic-layers thermal barrier coatings system”, Surface and Coatings Technology, v. 430, pp. 127989, 2022. doi: https://doi.org/10.1016/j.surfcoat.2021.127989.
» https://doi.org/10.1016/j.surfcoat.2021.127989 -
[25] TOLPYGO, V.K., CLARKE, D.R., MURPHY, K.S., “Oxidation-induced failure of EB-PVD thermal barrier coatings”, Surface and Coatings Technology, v. 146–147, pp. 124–131, 2001. doi: https://doi.org/10.1016/S0257-8972(01)01482-7.
» https://doi.org/10.1016/S0257-8972(01)01482-7 -
[26] MUMM, D.R., EVANS, A.G., “On the role of imperfections in the failure of a thermal barrier coating made by electron beam deposition”, Acta Materialia, v. 48, n. 8, pp. 1815–1827, 2020. doi: https://doi.org/10.1016/S1359-6454(99)00473-5.
» https://doi.org/10.1016/S1359-6454(99)00473-5 -
[27] MUMM, D.R., EVANS, A.G., SPITSBERG, I.T., “Characterization of a cyclic displacement instability for a thermally grown oxide in a thermal barrier system”, Acta Materialia, v. 49, pp. 2329–2340, 2001. doi: https://doi.org/10.1016/S1359-6454(01)00071-4.
» https://doi.org/10.1016/S1359-6454(01)00071-4 -
[28] ZHAO, X., WANG, X., XIAO, P., “Sintering and failure behaviour of EB-PVD thermal barrier coating after isothermal treatment”, Surface and Coatings Technology, v. 200, n. 20–21, pp. 5946–5955, 2006. doi: https://doi.org/10.1016/j.surfcoat.2005.09.006.
» https://doi.org/10.1016/j.surfcoat.2005.09.006 -
[29] ZHAO, X., XIAO, P., “Residual stresses in thermal barrier coatings measured by photoluminescence piezospectroscopy and indentation technique”, Surface and Coatings Technology, v. 201, n. 3–4, pp. 1124–1131, 2006. doi: https://doi.org/10.1016/j.surfcoat.2006.01.035.
» https://doi.org/10.1016/j.surfcoat.2006.01.035 -
[30] LIUYU, Y., DINGJUN, L., et al, “Simultaneous measurement of TGO thickness and residual stress in thermal barrier coating system via extension of PLPS method”, Journal of Alloys and Compounds, v. 1024, pp. 179972, 2025. doi: https://doi.org/10.1016/j.jallcom.2025.179972.
» https://doi.org/10.1016/j.jallcom.2025.179972 -
[31] NEU, R.W., SEHITOGLU, H., “Thermomechanical fatigue, oxidation, and creep: Part II—Life prediction”, Metallurgical Transactions. A, Physical Metallurgy and Materials Science, v. 20, n. 9, pp. 1769-1783, 1989. doi: https://doi.org/10.1007/BF02663208.
» https://doi.org/10.1007/BF02663208 -
[32] CHEN, X., HE, M.Y., SPITSBERG, I., et al., “Mechanisms governing the high temperature erosion of thermal barrier coatings”, Wear, v. 256, n. 7–8, pp. 735–746, 2021. doi: https://doi.org/10.1016/S0043-1648(03)00446-0.
» https://doi.org/10.1016/S0043-1648(03)00446-0 -
[33] HILLE, T.S., NIJDAM, T.J., SUIKER, A.S.J., et al., “Damage growth triggered by interface irregularities in thermal barrier coatings”, Acta Materialia, v. 57, n. 9, pp. 2624–2630, 2009. doi: https://doi.org/10.1016/j.actamat.2009.01.022.
» https://doi.org/10.1016/j.actamat.2009.01.022 -
[34] BOGDAN, M., PETER, I., “A Comprehensive understanding of Thermal Barrier Coatings (TBCs): applications, materials, coating design and failure mechanisms”, Metals, v. 14, n. 5, pp. 575, 2024. doi: https://doi.org/10.3390/met14050575.
» https://doi.org/10.3390/met14050575 -
[35] IQBAL, A., MOSKAL, G., “Recent development in advance ceramic materials and understanding the mechanisms of thermal barrier coatings degradation”, Archives of Computational Methods in Engineering, v. 30, n. 8, pp. 4855-4896, 2023. doi: https://doi.org/10.1007/s11831-023-09960-7.
» https://doi.org/10.1007/s11831-023-09960-7 -
[36] IQBAL, A., MOSKAL, G., CAVALEIRO, A., et al., “The current advancement of zirconate based dual phase system in thermal barrier coatings (TBCs): New modes of the failures: Understanding and investigations”, Alexandria Engineering Journal, v. 91, pp. 161–196, 2024. doi: https://doi.org/10.1016/j.aej.2024.01.063.
» https://doi.org/10.1016/j.aej.2024.01.063 -
[37] YAN, W., LI, C., ZHOU, Q., et al., “Uncertainty quantification of thermal barrier coatings lifetime on rotating turbine blades considering chemo-thermo-mechanically coupling failure”, Materials & Design, v. 253, pp. 113878, 2025. doi: https://doi.org/10.1016/j.matdes.2025.113878.
» https://doi.org/10.1016/j.matdes.2025.113878 -
[38] ASHOFTEH, A., RAJABZADEH, M., “Advances in thermal barrier coatings modeling, simulation, and analysis: A review”, Journal of the European Ceramic Society, v. 44, n. 14, pp. 116693, 2024. doi: https://doi.org/10.1016/j.jeurceramsoc.2024.116693.
» https://doi.org/10.1016/j.jeurceramsoc.2024.116693 -
[39] TANG, W.Z., YANG, L., ZHU, W., et al., “Numerical simulation of temperature distribution and thermal-stress field in a turbine blade with multilayer-structure TBCs by a fluid-solid coupling method”, Journal of Materials Science and Technology, v. 32, n. 5, pp. 452–458, 2016. doi: https://doi.org/10.1016/j.jmst.2016.03.009.
» https://doi.org/10.1016/j.jmst.2016.03.009 -
[40] XU, G.N., YANG, L., ZHOU, Y.C., et al., “A chemo-thermo-mechanically constitutive theory for thermal barrier coatings under CMAS infiltration and corrosion”, Journal of the Mechanics and Physics of Solids, v. 133, pp. 103710, 2019. doi: https://doi.org/10.1016/j.jmps.2019.103710.
» https://doi.org/10.1016/j.jmps.2019.103710