ABSTRACT
This research investigates the influence of quartz sand and alccofine on the mechanical and durability performance of concrete. Quartz sand was used to replace natural fine aggregate in various percentages (0%, 25%, 50%, 75%, and 100%), while alccofine was added as a replacement to cement by 10%. The experimental plan consisted of testing for compressive, split tensile, and flexural strength and durability tests under hydrochloric acid and sulfuric acid exposure. The test results indicated that mix AQ25, consisting of 25% quartz sand and 10% alccofine, was the best performing mix, with a 28-day compressive strength of 61.27 MPa, which is an increase of 38% over conventional concrete. Mix AQ25 also resulted in higher values of split tensile (3.52 MPa) and flexural strength (6.3 MPa), reflecting improved characteristics of ITZ. Tests for acid resistance also demonstrated a higher residual strength and less deterioration for quartz sand-based mixes, with AQ25 maintaining strengths of 59.55 MPa after 1% HCl and 53.25 MPa after 1% H2SO4 attack. SEM observations also showed improved microstructural density, superior formation of C-S-H gel, and reduced porosity for optimized mixes. In general, the blending of alccofine with 25% quartz sand increases the strength and durability of concrete considerably.
Keywords:
Alccofine; quartz sand; strength; durability; SEM analysis
1. INTRODUCTION
Concrete is one of the most used construction materials all over the world, and cement is its most critical component [1]. On the other hand, the manufacturing process of cement gives rise to a significant amount of carbon dioxide (CO2) emissions and is responsible for nearly 7% of the GHG emissions of the world. Of all the GHGs, the emission of CO2 from the energy sector is pretty substantial [2, 3]. At the same time, industrial activities are producing an increasing amount of wastes. These reasons have made the concrete sector, in recent years especially in the last ten years, shift toward sustainability by using SCMs [4]. SCMs, which can replace cement partially or fully, are gaining popularity due to their capability to improve long-term mechanical performance, durability, and sustainability [5]. Alccofine, a microfine mineral additive, is a new type of slag-based SCM. It is mainly available in two series: the 1200 series and the 1100 series. The numerical grades 1201, 1202, and 1203 represent the fine, microfine, and ultrafine particle sizes, respectively. Alccofine 1101 has a microfine size with a high C-S-H content and is employed for grouting, rock anchoring, and soil stabilization [6]. Alccofine 1203 is an environment-friendly and highly reactive material with a high content of glass, having a specific fineness of 12,000 cm2/g. Researches showed that replacing Portland pozzolana cement by alccofine and fine aggregate by foundry slag has the potential to develop high-performance concrete with minimal environmental impact and preservation of natural resources [7]. In this respect, the alccofine-based geopolymer concrete exhibited enhanced densification, strength, and microstructural properties, thus proving to be an eco-friendly alternative in modern concrete applications [8, 9].
The addition of alccofine improves concrete workability through a reduction in the total water demand. Among both the control mix and the other alccofine-based blends, the maximum compressive, flexural, and split tensile strengths were observed at 7, 28, and 56 days with the partial replacement of cement by 20% fly ash and 10% alccofine [10, 11]. High pozzolanic reactivity of alccofine results in the formation of a dense C-S-H gel, which is the main reason for a great improvement in compressive strength [12]. Strength gain is rapid at the early stages of curing and continuous at later ages, and optimum strength was observed at a 10% replacement of alccofine [13]. Such a replacement gives better pore structure and particle packing, thereby allowing for mechanical properties to be enhanced by up to 20% compared with conventional cement mixes. Such alccofine microparticles make the ITZ denser, which is favorable for increased concrete strength [14]. Sulfuric acid is very aggressive towards concrete due to the strong reactivity of sulfuric acid towards free lime in the form of gypsum. Such gypsum further reacts with calcium aluminates to form ettringite, which has very low solubility [15]. The extreme expansion of these resulting products produces internal pressure leading to crack development in the concrete matrix [16, 17]. These insoluble compounds, through their accumulation in pore spaces, weaken the bond between cement paste and aggregates and cause strength reduction, expansion, and microcracking [18].
SEM and XRD reveal that alccofine reduces the porosity in the microstructure and increases the generation of Ca2O4Si and C- (A-)S-H [19]. SEM tests also show the growth of ettringite needles and C-S-H gel in voids [20]. The concrete develops maximum compressive strength at 10% replacement of alccofine, which demonstrates a rapid strength gain in the first seven days and gradual development up to 28 days [21]. Also, alccofine improves various self-compacting properties such as resistance to segregation, filling, and passing abilities with lower costs compared to cement [22]. Compressive and flexural strengths resulting from alccofine were higher in both river sand and manufactured sand mixes. Alccofine exhibited the highest value of flexural strength among alccofine, metakaolin, and silica fume, with a 21% increase in strength for manufactured sand mixes over conventional concrete. The flexural strength at 56 days was 12% more compared to the strength at 28 days [23, 24]. Compressive strength was maximum for the combination of 30% glass powder and 10% alccofine replacement with a 28-day strength of 81.60 MPa at a w/c ratio of 0.26 for standard concrete - 80.52 Mpa [25]. Flexural strength at 28 days was also significantly higher, at 7.29 MPa versus 6.15 MPa for regular concrete [26]. Moreover, the combined use of alccofine and zinc oxide has been shown to enhance both the strength and durability of cured concrete [27].
Natural river sand is using extensively as a fine aggregate due to the increasing demand for concrete, which lowers river water tables and results in the exploitation of this natural resource [28]. River sand, which is used as an fine aggregate in concrete is becoming increasingly scarce which opens the door for the construction sector to look for alternatives [23]. The most prevalent material in the Earth’s crust is quartz [29]. Pure quartz is transparent and colourless. Although it is found in nearly all sedimentary, metamorphic rocks, in igneous rocks. Silica is its base and its formula is SiO2. On the Mohrs hardness scale, it is a 7. It has been known for being exceptionally strong to both mechanical and chemical conditions [30]. Under the chosen aggressive conditions (HCl and H2SO4), measurable deterioration and meaningful residual strength differences were already observed at 28 days, allowing reliable differentiation between mixes particularly the superior performance. [31] While this duration provides useful insight into the comparative behaviour of the mixes, we agree that it does not fully capture long-term degradation mechanisms. Therefore, a statement clarifying this limitation has been added to the revised manuscript [32]. Despite these benefits, as there is limited research on using quartz sand in conjunction with alccofine in this task, an attempt has been made to determine the ideal ratio of quartz sand to replace sand in concrete and alccofine as a substitute for cement. Further, the study sought to determine how alccofine and quartz sand affected mechanical and durability qualities.
2. MATERIALS AND METHODS
The materials used in this investigation include cement, alccofine 1203, river sand, quartz sand, coarse aggregate, superplasticizer, and water.
2.1. Cement
Ordinary Portland Cement 53 grade, which complies with IS 12269 requirements, is the preferred cement [31]. The specific gravity is 3.15 and its fineness is 4.48%, which is less than 10% according to IS 4031 part1 [32]. EDX spectrum displays the elemental composition of OPC shown in Figure 1. The calcium (CaK- 47.94 %) were found utmost quantity compared to other elements in OPC from EDX spectrum. Where k factor (K electrons, closest to the nucleus, are n = 1 electrons) represents the net-count ratios of characteristic or intensity X-rays of sample measurement divided by standard of known or reference sample [33].
2.2. Fine aggregate
River sand is widely used in construction for its excellent workability and compatibility with cementitious mixes. The grainy texture provides smooth finishes and interlocking, while a specific gravity of 2.62 offers stability and compaction. With low water absorption at 1%, it maintains mix consistency. Classified as Zone II, it provides a good, balanced gradation for general applications, hence ideal for strength, durability, and performance.
2.3. Coarse aggregate
The physical and chemical properties of the coarse particles play an influential role in the strength, durability, and overall performance of concrete. Aggregates of 20 mm size, which are angular in shape, used in this study have a bulk density of 1634 kg/m3 and a specific gravity of 2.72, hence providing stability and proper compaction within the concrete matrix. These aggregates possess excellent resistance to loads, impacts, and structural strains, as was deduced from their water absorption rate of 0.5%, crushing value of 16.99%, and impact strength of 14.41%.
2.4. Alccofine
Alccofine used in this study falls under the category of Alccofine 1203, conforming to the requirements specified in IS 12089–1987 [34] and IS 456–2009 [35]. Alccofine 1203 is an ultra-fine, white slag with a specific gravi-ty of 2.86 and particle size falling between 4–6 µm, obtained from a local supplier. Energy Dispersive X-ray (EDX) spectrum analysis shows that Alccofine contains maximum proportions of calcium (CaK) as 28.28% and active silica (SiK) as 15.04% among other elements, as shown in Figure 2. These attributes make it a highly reactive and efficient supplementary cementitious material.
2.5. Quartz sand
Quartz sand is a natural mineral obtained by crushing and grinding quartz stone. Quartz sand plays a vital role in numerous industrial and technological fields. It has diverse functions and is an indispensable raw material for many industries. There are two basic components to quartz sand: silica and oxygen. Quartz can be found in a variety of shades and is typically white or colorless. It is also referred to as silica sand, white sand, or industrial sand. Each sand deposit’s color is mostly determined by the variety of minerals and rock debris that comprise the resource. The elemental compositions of quartz sand from EDX spectrum is shown in Figure 3. It displays the presence of active silica (SiK-36.95 %) and oxygen (63.05%). Natural river sand, quartz sand is used as fine aggregates (Zone-II) and coarse aggregates according to IS 383-2016 [36].
2.6. Superplasticizer
La Hyper Crete S20 is an advanced hyperplasticizer developed from modified polycarboxylic ether, primarily used to enhance and retain concrete workability, in accordance with IS 9103:1999 [37]. This superplasticizer has a specific gravity of 1.08, and its dosage is determined based on the requirements of the mix design. Potable water is employed in concrete preparation, while curing practices are carried out as per the guidelines specified in IS 456:2009 [35].
3. METHODOLOGY
The mix design for M35 grade concrete was carried out in accordance with IS 10262:2019 [38] and IS 456:2009 [35]. The obtained weight proportions were 1:1.588:3.00:0.0055:0.38 for cement, fine aggregate, coarse aggregate, superplasticizer, and water, respectively. After control mix, 10% of alccofine was used to substitute cement and Quartz sand (0, 25, 50, 75 and 100%) was used to replace sand. First, the required quantity of cement, alccofine, river sand and quartz sand were mixed dry till a uniform mix was obtained and then the content was added to the coarse aggregate in the mixer. Initially, the concrete ingredients were allowed for dry mixing, further necessary amount of water, superplasticizer was included slowly and blended to obtain the concrete with the required consistency. For easy detaching, oil was applied to the inner faces of mould. The moulds were filled with concrete to prepare test specimens. Cube 100 × 100 × 100 mm, 100 mm dia by 200 mm height cylinder specimen and 100 × 100 × 500 mm beam specimen is used. The casted specimens removed from the mould after a day and allowed to cure in water for 7, 14 and 28 days.
To ensure accuracy in the test results, for compressive strength the cubes were cleaned to eliminate any loose sand or particles. They were then placed inside the testing apparatus, and the load was progressively applied at a fixed rate of about 140 kg/cm2/min until failure happened. The cylinder specimen placed horizontally between loading surfaces. A constant load of 1.4 MPa/min was supplied without causing any shock. The test was continued until it failed and the highest load at failure was recorded. The beam was set up horizontally on 300 mm-apart rollers. Until failure, two point loads were applied. Subsequently, the acid resistance of seventy-two cubes measured 100 mm by 100 mm by 100 mm was assessed. Each value represents the average outcome of three specimens from the same group. The methodology was aligned with ASTM C267 for acid exposure, while sample preparation and strength testing followed IS 516. The 1% and 5% HCl and 1% and 5% H2SO4 solutions were monitored weekly for pH variation and refreshed every 7 days to maintain consistent aggressiveness throughout the 28-day immersion. The specimens were taken out, their masses determined, and their surfaces dried after a period of 28 days. Curves are created by plotting the % of quartz sand on the X-axis and the ratio of the compressive strength of the Alccofine, Quartz Sand concrete to the the compressive strength strength of control mix concrete on the Y-axis. Curves are generated as well for flexural strength, splitting tension strength. Images from SEM are used to assess the concrete’s microstructure. Figure 4 experimental programs of various test. Table 1 shows the mix propositions.
4. RESULTS AND DISCUSSION
4.1. Compressive strength test
Figure 5 findings for the various concrete mixes’ compressive strengths at 7, 14, and 28 days. The control mix (CC) obtained compressive values of 35 MPa, 40.31 MPa, and 44.3 MPa, respectively, indicating baseline performance without alccofine or quartz sand. The inclusion of 10% alccofine in AQ0 (no quartz sand replacement) significantly enhanced compressive strength across all ages, with values of 43.09 MPa, 50.72 MPa, and 55.74 MPa at 7, 14, and 28 days, respectively. The pozzolanic nature of alccofine, which densifies the concrete matrix. AQ25, with 25% quartz sand replacement, obtained the highest compressive strength: 46.6 MPa, 55.76 MPa, and 61.27 MPa at 7, 14, and 28 days. Optimized particle packing and improved ITZ density accounted for this. AQ50 had slightly lower strength than AQ25 but was still higher than AQ0, obtaining 42.28 MPa, 52.42 MPa, and 57.6 MPa. The partial substitution of sand by quartz probably balanced matrix densification with workability. AQ75 and AQ100 showed a drop in compressive strength, while AQ100 attained a strength of 36.67 MPa, 50.51 MPa, and 55.5 MPa at 7, 14, and 28 days. The excess amount of quartz sand probably disrupted the optimal gradation and resulted in reduced co-hesion and performance. Generally, it has been seen that the addition of alccofine coupled with 25% replacement of quartz sand yielded the maximum compressive strength, as observed, and hence could have wider applications in the realm of sustainable high-performance concretes.
4.2. Split tensile strength
The split tensile strength results of all mixes at 7, 14, and 28 days are presented in Figure 6. The results indicate a consistent increase in tensile strength with curing age for all mixtures. At 7 days, the control mix (CC) exhibited a strength of 2.16 MPa. With the incorporation of quartz sand and alccofine, the strength improved, reaching a maximum of 2.54 MPa for AQ25. AQ50 showed 2.45 MPa, while AQ75 and AQ100 recorded 2.36 MPa and 2.33 MPa, respectively. At 14 days, a similar trend was observed. CC attained 2.74 MPa, whereas AQ25 achieved the highest strength of 3.21 MPa. AQ50 followed with 3.10 MPa, and AQ75 and AQ100 showed 2.98 MPa and 2.95 MPa, respectively. At 28 days, the tensile strength further increased for all mixes. The control mix recorded 3.00 MPa, while AQ25 achieved the highest value of 3.52 MPa. AQ50 reached 3.40 MPa, followed by AQ75 (3.27 MPa) and AQ100 (3.23 MPa). Although AQ0 (3.22 MPa) showed improvement over the control, the optimum performance was clearly observed at 25% quartz sand replacement. The improvement can be attributed to enhanced particle packing and matrix densification, which improve the interfacial transition zone (ITZ). However, beyond 25% replacement, a gradual reduction in tensile strength was observed, possibly due to disruption in optimal gradation and reduced cohesion within the matrix.
4.3. Flexural strength test
Figure 7 presents the flexural strength development of concrete mixes at curing age 7, 14, and 28 days. The control mix (CC), having no alccofine and quartz sand incorporation, recorded flexural strengths of 2.62 MPa, 3.66 MPa, and 4.03 MPa, respectively. Mix AQ0, comprising 10% alccofine without quartz sand replacement, demonstrated marked improvement, with flexural strength values of 3.47 MPa, 4.86 MPa, and 5.35 MPa at the respective ages. Such enhancement is primarily due to the pozzolanic reactivity of alccofine, which refines the matrix and enhances resistance against crack propagation. Among all the mixes, AQ25 showed the highest flexural strength, and was recorded at 4.09 MPa, 5.73 MPa, and 6.30 MPa at 7, 14, and 28 days, respectively. The better performance of AQ25 is due to the synergetic effect of the filler properties of alccofine with the optimized quartz sand content, which improves the densification of the matrix and strengthens the ITZ, leading to better flexural capacity. AQ50 resulted in strengths slightly lower than that of AQ25, with strengths of 3.83 MPa, 5.37 MPa, and 5.91 MPa, respectively. Increased quartz sand content may lead to reduced homogeneity of the mix, affecting the load-carrying and distribution aspects. AQ75 and AQ100 resulted in further reductions in flexural strength, and AQ100 recorded a strength of 3.51 MPa, 4.92 MPa, and 5.41 MPa, respectively. Unduly higher replacement of quartz sand might cause disruption in proper aggregate gradation and bonding within the matrix. The results depict that the optimum combination for flexural strength is with 10% Alccofine and 25% quartz sand replacement, which maximizes strength and durability of the matrix.
4.4. Comparison of strength of Alccofine, Quartz sand concrete with conventional concrete
Adding Alccofine and quartz sand to concrete had the effect of greatly strengthening the concrete when compared to a control mix, CC. Table 2 represents comparison of strength of Alccofine, Quartz sand concrete with Conventional Concrete. Compressive strength ratios increased by 26% for AQ0, which is 10% Alccofine, to a maximum of 1.38 for AQ25, indicating that the best synergy of Alcco-fine was with 25% quartz sand. At values higher than this, ratios fell back somewhat: for AQ50, AQ75, and AQ100, values of 1.30, 1.26, and 1.25, respectively, were achieved. The Flexural strength ratio followed a similar trend: AQ0, at 33% improvement, reflected increased resistance to bending, while AQ25 reached a maximum of 1.56 due to ITZ refinement. For AQ50, there was a moderate increase of 1.47, while the value for AQ75 fell off further, to 1.37, and that for AQ100 to 1.34. Split tensile strength ratios improved modestly to a maximum of 1.07 for AQ0 and peaked at AQ25 to 1.17. However, higher quartz sand replacements led to gradual reductions, with AQ50, AQ75, and AQ100 achieving 1.13, 1.09, and 1.07, respectively. These results highlight the effectiveness of Alccofine in improving strength properties and demonstrate that the optimal combination is 10% Alccofine with 25% quartz sand, which provides the best balance across compressive, tensile, and flexural strengths. Figures 8, 9, and 10 illustrate how the proportion of quartz sand affects compressive, split tensile, and flexural strength.
4.5. Residual Compressive Strength of alccofine, quartz sand concrete after exposed to HCL
The residual compressive strength of alccofine and quartz sand concrete exposed to hydrochloric acid (HCl) quantifies the performance of this concrete under aggressive chemical environments. At 1% HCl concentra-tion, the residual strength for the control mix (CC) was 39.12 MPa, significantly lower than mixes with alccofine, Quartz sand. AQ0 achieved 51.84 MPa, and AQ25 showed the highest resistance with 59.55 MPa, indicating enhanced durability with 25% quartz sand replacement. AQ50, AQ75, and AQ100 recorded strengths of 56.12 MPa, 54.35 MPa, and 54.12 MPa, respectively. At 5% HCl, the control mix exhibited a marked reduction to 35.45 MPa, while AQ0 retained 38.13 MPa. AQ25 again achieved su-perior performance with 49.35 MPa, reflecting its optimal chemical resistance. AQ50, AQ75, and AQ100 demonstrated residual strengths of 41.88 MPa, 40.23 MPa, and 39.78 MPa, respectively. In fact, these results have pointed out the function of alccofine and quartz sand in mitigating the effects of acidic attack, with the AQ25 mix offering the most balanced performance. Figure 11 residual compressive strength of concrete after exposed to HCL at 28 days.
4.6. Residual compressive strength of alccofine, quartz sand concrete after exposed to H2SO4
The residual compressive strength of Alccofine and quartz sand concrete exposed to sulfuric acid (H2SO4) underlines the resistance offered to chemical degradation. For 1% H2SO4 concentration, CC retained a strength of 35.74 MPa, while AQ0 exhibited a marginal improvement at 40.14 MPa. AQ25 attained a maximum resistance value of 53.25 MPa by demonstrating the advantage of incorporating 25% quartz sand. AQ50, AQ75, and AQ100 recorded residual strengths of 48.32 MPa, 45.34 MPa, and 41.25 MPa, respectively. Under the more aggressive 5% H2SO4 exposure, the control mix’s strength reduced significantly to 15.28 MPa. AQ0 slightly outperformed it with 16.56 MPa, while AQ25 again demonstrated superior performance at 19.33 MPa. AQ50, AQ75, and AQ100 achieved residual strengths of 17.46 MPa, 17.19 MPa, and 17.02 MPa, respectively. The results indicate that Alccofine and quartz sand improve acid resistance, with the AQ25 mix proving most effective against sulfuric acid attack. Figure 12 residual compressive strength of concrete after exposed to H2SO4 at 28 days
4.7. Mass loss of alccofine, quartz sand concrete after exposed to HCL & H2SO4
The percentage of mass loss due to acid exposure varies depending on the concentration of the acid and the mix composition. For 1% HCl, the mass loss ranged from 0.36% to 0.79%, while for 5% HCl, it is increased, varying between 1.54% and 1.96%. Similarly, for 1% H2SO4, the mass loss for all mixes ranged from 0.38% to 1.16%, whereas exposure to 5% H2SO4 resulted in significantly higher mass losses, varying between 15.48% and 17.97%. The enhanced resistance of quartz sand concrete to sulfuric acid attack can be attributed to the highly siliceous nature of quartz sand. Quartz, being chemically inert, reacts with acid at a much slower rate compared to hydrated cement stone, thereby reducing the overall mass loss in acid-exposed concrete.
4.8. Ratio of compressive strength of concrete with Alccofine, quartz sand and compressive strength of conventional concrete at 0, 1% and 5% HCL
The addition of 10% alccofine as cement replacement increased strength in all mixes considerably. Control concrete mixture, CC, was taken as reference with the ratio of compressive strength to be 1.00 at all conditions. The compressive strength ratio for mixture AQ0 (10% alccofine, 0% quartz sand) was 1.26 at normal conditions, 1.33 after 1% HCl attack, and 1.08 under 5% HCl attack. This proves that alcco-fine is resistant against acid attack. For mixture AQ25 (10% alccofine, 25% quartz sand), the highest compressive strength ratios were recorded at all conditions, namely 1.38 at normal, 1.52 after 1% HCl attack, and 1.39 after exposure to 5% HCl attack, reflecting the syner-gistic contributions in resisting chemical degradation when alccofine is combined with quartz sand. There was a slight drop in the strength ratios in mixes containing a higher percentage of quartz sand replacements. For AQ50, the compressive strength ratios were 1.30, 1.43, and 1.18, while the compressive strength ratios of AQ75 and AQ100 mixes remained sufficiently encouraging, ranging from 1.12 to 1.26. These observations revealed that alccofine enhances the microstructure by forming dense C-S-H while the quartz sand imparts superior acid resistance due to its high silica content. Table 3. The ratio of compressive strength of concrete with alccofine, quartz sand and strength of concrete without having alccofine, quartz sand for 0, 1, 5% HCL at 28 days of curing. Table 3. The ratio of compressive strength of concrete with alccofine, quartz sand and strength of con-crete without having alccofine, quartz sand for 0, 1, 5% HCL at 28days of curing. Overall, the combination of 10% alccofine and 25% quartz sand (AQ25) was the best in that respect, offering improved strength and durability under normal and aggressive chemical environments, respectively. Hence, it may be considered a potential option towards sustainable high-performance concretes.
The ratio of compressive strength of concrete with alccofine, quartz sand and compressive strength of concrete without having alccofine, quartz sand for 0, 1, 5% HCL at 28 days of curing.
4.9. Ratio of compressive strength of concrete with alccofine, quartz sand and compressive strength of conventional concrete at 0, 1%, 5% H2SO4
In general, the addition of alccofine and quartz sand into concrete significantly improved the resistance to sulfuric acid attack as reflected in the ratios of compressive strengths fcaq/fco, fS1caq/fS1co, and fS5caq/fS5co. For 0% H2SO4 exposure, all the mixes with alccofine exhibited higher strength than the control mix, CC. For AQ25, the ratio was 1.38 and for AQ50 it was 1.30. This could be explained by the fact that the addition of alccofine and quartz sand caused a refinement in microstructure, which helped in producing a denser matrix. For mixes exposed to 1% H2SO4, the same trend was observed, with AQ25 having the best acid resistance with a strength ratio of 1.49, indicating that when both alccofine and quartz sand are combined, there is a synergistic effect on mitigating the degradation of concrete due to acid attack. Though the performance of AQ50 and AQ75 was slightly lower, their performances were still better than that of the control mix, proving that these two additives are effective in reducing acid damage to concrete.
Under the more aggressive 5% H2SO4 exposure, the strength ratios decreased for all mixes, indicating the severity of the acid’s attack. However, AQ25 again showed better resistance with a ratio of 1.27, followed by AQ50 at 1.14. The degradation at higher acid concentration may be explained by the progressive dissolution of calcium silicate hydrates and leaching of calcium compounds. Table 4 the ratio of compressive strength of concrete with alccofine, quartz sand and strength of concrete without having alccofine, quartz sand for 0, 1, 5% H2SO4 at 28 days of curing. In general, it can be outlined from the test results that alccofine and quartz sand enhance the acid resistance of concrete, and amongst them AQ25 performs better. Such observations delineate the promising role of these materials in enhancing the durability of concrete in acidic environments.
The ratio of compressive strength of concrete with alccofine, quartz sand and compressive strength of concrete without having alccofine, quartz sand for 0, 1, 5% H2SO4 at 28 days of curing.
4.10. SEM analysis
The SEM micrographs give information on the microstructural aspects of concrete mixes with and without alccofine and also on varying percentages of quartz sand. The control mix, CC, Figure 13a, presents large voids and an irregular matrix, indicative of weaker bonding and higher porosity. The presence of CH crystals is very pronounced, which can eventually lead to reduced durability in aggressive environments.
In AQ0 (Figure 13b), the addition of 10% alccofine shows a marked improvement in the microstructure. There is a formation of C-S-H gel and reduced voids, enhancing the density and strength of the matrix. AQ25 (Figure 13c) exhibits the best microstructure among all mixes. Replacement of sand partially by 25% quartz sand, along with alccofine, has yielded a denser and more homogeneous matrix. The plentiful formation of C-S-H gel and improved ITZ reflects better bonding and reduced porosi-ty, which could be responsible for better mechanical and durability properties.
In contrast to AQ25, the microstructure in AQ50 (Figure 13d) is still dense, but there are a few small voids. There are few CH crystals present, demonstrating strong mechanical and acid resistance qualities. In AQ75 (Figure 13e) and AQ100 (Figure 13f), further replacement of sand with quartz sand results in a slight increase in voids. Nonetheless, the micrographs show a uniform distribution of C-S-H gel, preserving sufficient matrix bonding. Alccofine and ideal quartz sand replacement greatly improve microstructure, decrease porosity, and increase the strength and durability of the concrete, according to the SEM analysis.
5. CONCLUSION
-
This paper presents the novel combined use of quartz sand as fine aggregate replacement and 10% alccofine as cement substitute, showing remarkable improvements in both mechanical performance and acid resistance when compared to conventional concrete.
-
AQ25 – 25% quartz sand + 10% alccofine - was found to be the optimum mix, which recorded the highest 28-day compressive strength of 61.27 MPa that was 38% higher than the control, and exhibited the best split tensile of 3.52 MPa and flexural strength of 6.3 MPa due to improved packing density and a denser ITZ.
-
Quartz-sand-modified mixes showed improved acid resistance: AQ25 had a residual strength of 59.55 MPa in 1% HCl and 53.25 MPa in 1% H2SO4, showing significantly lower deterioration compared with the control mix. The siliceous nature of quartz sand was beneficial in hindering acid-induced degradation.
-
SEM analysis shows microstructural refinement with reduced voids, denser C-S-H formation, and a more cohesive matrix in the optimized mix, which correlates directly to improvements in strength and durability.
-
Practical Implication: The addition of 25% quartz sand with 10% alccofine presents an appropriate solution for a sustainable high-performance concrete intended for structures subjected to highly aggressive chemical attack and applications with enhanced durability and mechanical efficiency.
6. BIBLIOGRAPHY
-
[1] BOOBALAN, S., SRIVATSAV, V.A., NISATH, A.M.T., et al, “A comprehensive review on strength properties for making Alccofine based high performance concrete”, Materials Today: Proceedings, v. 45, pp. 4810–4812, 2021. doi: https://doi.org/10.1016/j.matpr.2021.01.278.
» https://doi.org/10.1016/j.matpr.2021.01.278 -
[2] BELMOKADDEM, M., MAHI, A., SENHADJI, Y., et al, “Mechanical and physical properties and morphology of concrete containing plastic waste as aggregate”, Construction & Building Materials, v. 257, pp. 119559, 2020. doi: https://doi.org/10.1016/j.conbuildmat.2020.119559.
» https://doi.org/10.1016/j.conbuildmat.2020.119559 - [3] ANBARASU, N.A., KESHAV, L., KALYANA, C.P.R., et al, “Unraveling the flexural behavior of concrete and compare with innovative fea investigations”, Materia, v. 29, n. 4, e20240656, 2024.
-
[4] BISWAS, R., RAI, B., “Efficiency concepts and models that evaluates the strength of concretes containing different supplementary cementitious materials”, Civil Engineering Journal, v. 5, n. 1, pp. 18–32, 2019. doi: https://doi.org/10.28991/cej-2019-03091222.
» https://doi.org/10.28991/cej-2019-03091222 -
[5] JUENGER, M., PROVIS, J.L., ELSEN, J., et al, “RAI, B., “Supplementary cementitious materials for concrete: characterization needs”, MRS Proceedings, v. 1488, pp. 8–22, 2012. doi: https://doi.org/10.1557/opl.2012.1536.
» https://doi.org/10.1557/opl.2012.1536 -
[6] SRINATH, B.S., PATNAIKUNI, C.K., BALAJI, K., et al, “A prospective review of alccofine as supplementary cementitious material”, Materials Today: Proceedings, v. 47, pp. 3953–3959, 2021. doi: https://doi.org/10.1016/j.matpr.2021.03.719.
» https://doi.org/10.1016/j.matpr.2021.03.719 -
[7] SHARMA, D., SHARMA, S., GOYAL, A., “Utilization of waste foundry slag and alccofine for developing high strength concrete”, International Journal of Electrochemical Science, v. 11, n. 4, pp. 3190–3205, 2016. doi: https://doi.org/10.1016/S1452-3981(23)16174-8.
» https://doi.org/10.1016/S1452-3981(23)16174-8 - [8] AKSHAY, H.S., KISHAN, A., KSHIRSAGAR, S., “Use of Alccofine 1203 in concrete roads”, International Journal of Applied Engineering Research: IJAER, v. 13, n. 7, pp. 299–301, 2018.
-
[9] CHINNUSAMY, B.S., VENKATARAMAN, G., “A comparative analysis of high-performance concrete: evaluation of strength and durability parameters with alternate fine aggregates and alccofine through response surface methodology model”, Matéria, v. 29, n. 3, e20240021, 2024. doi: https://doi.org/10.1590/1517-7076-rmat-2024-0021.
» https://doi.org/10.1590/1517-7076-rmat-2024-0021 -
[10] PRASAD BOKKA, D.V., SREE KUMAR, K., SUSEELA, K., et al, “Exploring the impact of alccofine and quarry dust on compressive and split tensile strength of concrete”, Journal of Physics: Conference Series, v. 2779, n. 1, pp. 012044, Jun. 2024. doi: https://doi.org/10.1088/1742-6596/2779/1/012044.
» https://doi.org/10.1088/1742-6596/2779/1/012044 -
[11] ANBARASU, N.A., SIVAKUMAR, V., YUVARAJ, S., et al, “Pioneering the next frontier in construction with high-strength concrete infused by nano materials”, Matéria, v. 30, e20240730, 2025. doi: https://doi.org/10.1590/1517-7076-rmat-2024-0730.
» https://doi.org/10.1590/1517-7076-rmat-2024-0730 - [12] KUMAR, S., SAMANTA, K., SINGHA ROY, K., “An experimental study on the mechanical properties of alccofine based high grade concrete”, International Journal of Multidisciplinary Research and Development, v. 2, n. 10, pp. 218-224, 2015.
-
[13] BHAT, A.H., NAQASH, J.A., “An experimental study on properties of concrete incorporating colloidal nanosilica and alccofine”, Innovative Infrastructure Solutions, v. 7, n. 3, pp. 196, 2022. doi: https://doi.org/10.1007/s41062-022-00800-4.
» https://doi.org/10.1007/s41062-022-00800-4 -
[14] ANNAMALAI, K., ANBARASU, N.A., GOVINDARAJAN, B.P., et al, “Sustainable concrete: integrating environmentally friendly materials for environmentally friendly construction”, Matéria, v. 30, e20250239, 2025. doi: https://doi.org/10.1590/1517-7076-rmat-2025-0239.
» https://doi.org/10.1590/1517-7076-rmat-2025-0239 - [15] UPADHYAY, S.P., JAMNU, “Effect on compressıve strength of hıgh performance concrete ıncorporatıng alccofıne and fly ash”, Journal of International Academic Research for Multidisciplinary, v. 2, n. 2, pp. 125–130, 2014. https://www.researchgate.net/publication/320078425, accessed in February, 2026.
-
[16] SAGAR, B., SIVAKUMAR, M.V.N., “Mechanical and microstructure characterization of alccofine based high strength concrete”, Silicon, v. 14, n. 3, pp. 795–813, 2022. doi: https://doi.org/10.1007/s12633-020-00863-x.
» https://doi.org/10.1007/s12633-020-00863-x -
[17] THANGAPANDI, K., ANURADHA, R., ARCHANA, N., et al, “Experimental study on performance of hardened concrete using nano materials”, KSCE Journal of Civil Engineering, v. 24, n. 2, pp. 596–602, 2020. doi: https://doi.org/10.1007/s12205-020-0871-y.
» https://doi.org/10.1007/s12205-020-0871-y -
[18] MUHEDIN, D.A., IBRAHIM, R.K., “Effect of waste glass powder as partial replacement of cement & sand in concrete”, Case Studies in Construction Materials, v. 19, e02512, 2023. doi: https://doi.org/10.1016/j.cscm.2023.e02512.
» https://doi.org/10.1016/j.cscm.2023.e02512 -
[19] ASHISH, D.K., VERMA, S.K., JU, M., et al, “High volume waste foundry sand self-compacting concrete: transitioning industrial symbiosis”, Process Safety and Environmental Protection, v. 173, pp. 666–692, 2023. doi: https://doi.org/10.1016/j.psep.2023.03.028.
» https://doi.org/10.1016/j.psep.2023.03.028 -
[20] RAFI, A., TASNIM, U., RAHMAN, M.S., “Quantification and qualification of silica sand extracted from padma river sand”, IOP Conference Series. Materials Science and Engineering, v. 438, pp. 012037, 2018. doi: https://doi.org/10.1088/1757-899X/438/1/012037.
» https://doi.org/10.1088/1757-899X/438/1/012037 -
[21] AYGÖRMEZ, Y., “Evaluation of the red mud and quartz sand on reinforced metazeolite-based geopolymer composites”, Journal of Building Engineering, v. 43, pp. 102528, 2021. doi: https://doi.org/10.1016/j.jobe.2021.102528.
» https://doi.org/10.1016/j.jobe.2021.102528 -
[22] MAHESWARAN, M., CHRISTY, C.F., MUTHUKANNAN, M., et al, “Parametric study on the performance of industrial byproducts based geopolymer concrete blended with rice husk ash & nano silica”, Research on Engineering Structures and Materials, v. 9, n. 4, pp. 1267–1285, 2023. doi: https://doi.org/10.17515/resm2023.809ma0703.
» https://doi.org/10.17515/resm2023.809ma0703 -
[23] ZHANG, P., GAO, Z., WANG, J., et al, “Properties of fresh and hardened fly ash/slag based geopolymer concrete: a review”, Journal of Cleaner Production, v. 270, pp. 122389, 2020. doi: https://doi.org/10.1016/j.jclepro.2020.122389.
» https://doi.org/10.1016/j.jclepro.2020.122389 -
[24] HASSAN, A., ARIF, M., SHARIQ, M., “Use of geopolymer concrete for a cleaner and sustainable environment: a review of mechanical properties and microstructure”, Journal of Cleaner Production, v. 223, pp. 704–728, 2019. doi: https://doi.org/10.1016/j.jclepro.2019.03.051.
» https://doi.org/10.1016/j.jclepro.2019.03.051 -
[25] HUANG, P., BAO, Y., YAO, Y., “Influence of HCl corrosion on the mechanical properties of concrete”, Cement and Concrete Research, v. 35, n. 3, pp. 584–589, 2005. doi: https://doi.org/10.1016/j.cemconres.2004.06.027.
» https://doi.org/10.1016/j.cemconres.2004.06.027 -
[26] AYDIN, S., YAZICI, H., YIGITER, H., et al, “Sulfuric acid resistance of high-volume fly ash concrete”, Building and Environment, v. 42, n. 2, pp. 717–721, 2007. doi: https://doi.org/10.1016/j.buildenv.2005.10.024.
» https://doi.org/10.1016/j.buildenv.2005.10.024 -
[27] KUMAR, S., NATARAJAN, M., NAVEEN ARASU, A., “A comprehensive microstructural analysis for enhancing concrete’s longevity and environmental sustainability”, Journal of Environmental Nanotechnology, v. 13, n. 2, pp. 368–376, 2024. doi: https://doi.org/10.13074/jent.2024.06.242584.
» https://doi.org/10.13074/jent.2024.06.242584 -
[28] ASHISH, D.K., VERMA, S.K., “Robustness of self-compacting concrete containing waste foundry sand and metakaolin: a sustainable approach”, Journal of Hazardous Materials, v. 401, pp. 123329, 2021. doi: https://doi.org/10.1016/j.jhazmat.2020.123329. PubMed PMID: 33113711.
» https://doi.org/10.1016/j.jhazmat.2020.123329 -
[29] SAJEEV, P.S., RAJAGOPAL, V.S.G., NAVEEN ARASU, A., “Investigation of concrete durability enhancement using supplementary cementitious materials”, MethodsX, v. 15, pp. 103527, 2025. doi: https://doi.org/10.1016/j.mex.2025.103527.
» https://doi.org/10.1016/j.mex.2025.103527 -
[30] SHARMA, H., ASHISH, D.K., SHARMA, S.K., “Development of low-carbon recycled aggregate concrete using carbonation treatment and alccofine”, Energy, Ecology & Environment, v. 9, n. 3, pp. 230–240, 2024. doi: https://doi.org/10.1007/s40974-023-00299-0.
» https://doi.org/10.1007/s40974-023-00299-0 - [31] BUREAU OF INDIAN STANDARDS, IS 12269:2013 Ordinary Portland Cement, 53 Grade – Specification, New Delhi, 2013.
- [32] BUREAU OF INDIAN STANDARDS, IS 4031 (Part 1) Indian Standard Method of Physical Tests for Hydraulic Cement, New Delhi, 1996.
- [33] SHANKAR, SAIRAM, S., NATARAJAN, M., et al, “Exploring the strength and durability characteristics of high-performance fibre reinforced concrete containing nanosilica”, Journal of the Balkan Tribological Association, v. 30, n. 1, 2024.
- [34] BUREAU OF INDIAN STANDARDS, IS:12089-1987 Indian Standard Specification for Granulated Slag for the Manufacture of Portland Slag Cement, New Delhi, 1987.
- [35] BUREAU OF INDIAN STANDARDS, IS 456-2009 Plain and Reinforced Concrete - Code of Practice, New Delhi, 2009.
- [36] BUREAU OF INDIAN STANDARDS, IS 383-2016, Indian Standard Specification for Coarse and Fine Aggregates from Natural Sources for Concrete, New Delhi, 2016.
- [37] BUREAU OF INDIAN STANDARDS, IS 9103:1999 Indian Standard Concrete Admixtures – Specification, New Delhi, 1999.
- [38] BUREAU OF INDIAN STANDARDS, IS 10262:2019, Concrete Mix Proportioning - Guidelines, New Delhi, 2019.