Abstract
The increasing release of gases that cause the greenhouse effect brings the need to develop products that minimize the environmental impact. In the civil construction sector, clinker, the main raw material for cement, releases large amounts of carbon dioxide during production. Thus, research related to geopolymers has stood out due to the lower release of gases into the atmosphere. Geopolymers are materials developed from aluminosilicates activated in a highly alkaline medium through geopolymerization. The compositions were prepared by varying the sodium hydroxide solutions NaOH (5, 7.5, and 10, Mols/L) and the proportions of sodium silicate Na2SiO3 to NaOH (1:2, 1:1 and 2:1) to determine a composition with the best characteristics. The factorial experiments of the type 3² were planned with 2 factors and 3 levels. The materials obtained were analyzed at 7 days of curing at room temperature. With the analysis of the results, it was possible to identify that the variation of the parameters SiO2/Al2O3 and Na2O/SiO2 have a significant influence. The Na2SiO3/NaOH ratio is the most important factor in the strength gain at early age. Compressive strength varied between 4.46 and 41.14 MPa as the smallest and highest SiO2/Al2O3 ratio, respectively.
Keywords:
geopolymer; metakaolin; compressive strength; optimization
INTRODUCTION
The study of alternative materials to Portland cement is a priority for research and an interest worldwide. The development of these new materials proposes to minimize greenhouse gas emissions to the atmosphere and achieve significant energy savings 1. The production of 1 ton of clinker, the main cement raw material, generates approximately 1 ton of carbon dioxide, or about 5 to 8% of world carbon dioxide emissions, making it a highly polluting material 1),(2. The geopolymer concrete production process reduces gas emissions by approximately 72% if compared to the conventional concrete production process, and with energy consumption that is reduced by about 46% during production 3, this data did not take into account the cost. In addition to the environmental context, it has already been shown that geopolymers can reach higher compressive strength, good chemical and thermal resistance, good aging properties, high-temperature resistance, and durability, which are beneficial for a high number of industrial applications 4),(5.
These materials, known as geopolymers, result from the polycondensation of aluminosilicates and alkaline solutions, producing three-dimensional polymeric structures 2),(6. Highly alkaline solutions such as NaOH and KOH are incorporated with source materials rich in SiO2 and Al2O36. For aluminosilicate-based geopolymers, the term poly (sialate) was suggested, where this sialate network consists of SiO4 and AlO4 tetrahedra alternately linked by oxygen sharing. Positive ions (Na+ or K+) are accommodated in the cavities of the structure to compensate for the negative excess charge of Al 3+ (4),(7. The most commonly used sources of aluminosilicate are metakaolin and fly ash 6),(8)-(10, the dissolution in alkaline media leads to the formation of individual alumina and silicate species that co-polymerize to form geopolymers 8. At the same time, sodium hydroxide (NaOH) is the most used alkaline activator due to its low cost, abundance, and lower viscosity 11. Compared to lower molarity, increasing the molarity of NaOH as an alkaline activator seems to increase compressive strength 12.
In research on geopolomerization, the material must be purer and more homogeneous, as is the case with metakaolin, while fly ash contains more impurities and hollow voids inside 10. Due to the disorder and X-ray amorphous nature 13)-(15, metakaolin has enormous reactive potential when in the presence of an alkaline solution 13. Metakaolin-based geopolymers microstructure can be conceptualized as a combination of partially reacted metakaolin compound, solid reaction product, and porous space, with the porous space filled with an aqueous alkaline solution 16.
The alkaline silicates are also commonly used in the production of geopolymers. The use of alkaline silicate activating solutions produces a product with lower crystallinity if compared to only alkaline hydroxides 14), (17. This is due to an increase in the reaction rate produced by the presence of soluble silicates 17), (18.
The ratios of the SiO2/Al2O3, Na2O/SiO2, and H2O/Na2O used for geopolymer preparation are essential for determining mechanical properties, and the results presented in the literature are limited and controversial 19. Thus, it is known that the increased SiO2/Al2O3 ratio causes the compressive strength to increase slightly 8),(19, while the H2O/Na2O molar ratio has a significant effect on the compressive strength, increasing this ratio causes a drastic drop in compressive strength due to the high porosity introduced by evaporation of water 19. The NaOH/Na2SiO3 ratio significantly impacts strength development 20. The Si/Al ratio is the most significant factor for the gain in compressive strength, as well as influencing the microstructure of the geopolymeric material 8. Ali, A.A. et al.21 found the maximum compressive strength at 28 days, about 64.7 MPa, which was optimal when the R ratio (SiO2/Al2O3) was around 3.6.
Geopolymers present a non-crystalline phase identified in X-ray diffractograms (XRD) by the presence of a “hump” in the range of 25 to 30° 17),(22. This hump is present in all geopolymers, regardless of the aluminosilicate source and activating solution, so it can be considered a distinctive feature of any geopolymer diffractogram, and its identification is essential in determining the microstructure of a geopolymer 17. There is data in the literature that characterizes the geopolymer binders as groups of nanocrystalline zeolites compacted by an amorphous gel phase, which can be observed through high-resolution microscopic techniques that the phase is nanoparticulated 17. To identify the changes that occur in the geopolymer formation structure, the FTIR spectra were used 22.
For microstructural analysis, the scanning electron microscope (SEM) and the transmission electron microscope (TEM) are often used. SEM analyses show microstructural changes in the material particles, causing changes in the geopolymeric phase, undissolved metakaolin, and the presence of pores in the matrix 23), (24. In TEM analysis, it is possible to observe the microstructure of the reagents, geopolymers, or polysialates. These are made up of nanoparticles separated by nanoporosity 25.
The present study aimed to explore the effects that occur on the microstructure and mechanical strength when variations are made in the molar proportions of the mixtures: SiO2/Al2O3, SiO2/Na2O, and H2O/Na2O. The concentration of the alkaline solution of NaOH and the proportions of sodium hydroxide to sodium silicate have been modified, resulting in variation in the relationships between SiO2/Na2O and SiO2/Al2O3. An experimental design was used to relate these molar ratios with the mechanical strength. This study innovates with Transmission Electron Microscopy (TEM) micrographs with images at a higher magnification, showing that the geopolymeric material produced is formed by clusters of small particles with nanometric size wrapped in a nanoporosity region. The diffraction pattern of the amorphous and crystalline geopolymer gel was found by TEM. A response surface curve of the mechanical property according to the ratios Na2.SiO3/NaOH and NaOH (mols/L) may be a contribution for researchers.
MATERIALS AND METHODS
The Metakaolin is a source of SiO2 and Al2O3 and was used for the preparation of the geopolymer mortar. Metacaulim do Brasil’s company was responsible for supplying this material, and Table 1 shows the composition of this material through X-ray fluorescence (Shimadzu EDX - 720). The mean particle size of metakaolin was 17.46 µm obtained by laser particle sizes analyzer (Shimadzu, SALD-2201) and presented 2.76 g/cm³ of density measured by gas pycnometer (Micromeritics, AccuPyc II 1340). The metakaolin was also analyzed by X-ray diffraction (Figure 1). The crystalline phases found in its composition were quartz (SiO2, PDF No. 01-079-1910), kaolinite (Al2Si2O5(OH)4, PDF No. 01-075-0938), and muscovite (H2KAl3SiO12, PDF No. 00-007-0032).
For the manufacture of the specimens, an experiment was planned with the aid of the software STATISTICA 8.0 to later analyze the effect of the variation SiO2/Al2O3 and SiO2/Na2O in the results of compressive strength obtained. The factorial experiments are of the type 3², where 2 stands for factors and 3 for levels. Four specimens were made for each composition, three of which were used for the compressive strength test and one for the XRD, FTIR, SEM, and TEM tests.
The preparation of specimens consisted of a few steps. Initially, the alkaline solution was prepared by dissolving sodium hydroxide micropearls (NaOH) with 99% purity (Reatec) in distilled water. The prepared solution remained at rest for 24 hours at room temperature once this is an exothermic reaction. The sodium silicate (Unaprosil), with the chemical composition of Na2O = 15.00%, SiO2 = 32.25%, and H2O = 53.75% by mass, was mixed with sodium hydroxide solution, and finally, the metakaolin was incorporated into the paste with the aid of a mechanical stirrer. The fresh paste was poured into PVC (polyvinyl chloride) cylindrical molds with dimensions of 25.0 mm x 50.0 mm and greased with Vaseline. The molds were covered with a glass plate to control water evaporation. The specimens were thickened for 20 seconds to reduce the number of voids and were cured inside a laboratory room with a temperature ranging from 20 to 25 ºC for 48h inside the mold. After this, the specimens remained at room temperature (20 to 25 ºC) until the day of the compressive strength test.
Keeping the same mass ratio of solids and liquids, a total of 9 metakaolin-based geopolymer mixtures were synthesized, as shown in Table 2. The mixtures were produced by changing the concentration of alkaline sodium hydroxide solution and the ratio of sodium silicate to the amount of NaOH solution. Initially, the samples were produced considering the ratio of 1:1 for solid/liquid based on initial laboratory experiments, where the solid is metakaolin, and the liquid is the alkaline solution. Then, it was determined to double the propositions (1:2 and 2:1) to verify the effects more clearly. With the response surface, it is possible to find results in the range of these variations. The percentages of NaOH and Na2SiO3 used and the molar concentrations of the NaOH solution are represented in Table 2 Görhan and Kürklü 26 also used the mass ratio of Na2SiO3/NaOH equal to 2.00, but with fly ash serving as precursor and addition of sand in the composition.
The proportions of the mixture components are presented in Table 3. To determine the consistency of the compositions, a 50 g sample of mixture was placed on the slumping table, and applying 20 blows, the spread of the mass was approximately 9.0 ± 0.5 cm for all mixtures.
The compressive strength was performed at 7 days of cure in a hydraulic press (EMIC, PC 220 I), according to the parameters described in NBR 7215 27. Three specimens were tested for each composition, in Table 2, only the values for mean and standard deviation were shown.
The microstructure was analyzed by a scanning electron microscope (SEM) and transmission electron microscope (TEM). The SEM analysis was done using a JEOL (JSM - 6701F). The samples were prepared with small parts of the initial specimens, and these were embedded in resin, sanded, polished, and covered with gold. For TEM analysis, which was performed with a JEOL (JEM - 2100), the specimens were ground to a nanometer grain size. Although geopolymers are amorphous, X-ray diffraction analysis (XRD) can be used to directly observe remaining crystalline phases during synthesis 28. For this analysis, the samples were ground and sieved in 250 mesh. The diffractometer (Shimadzu, XRD - 7000) with Cu radiation emissions was set with a scanning rate of 2°/min and a 2θ range of 5 - 80°.
The FTIR spectra were measured with a vacuum spectrometer (Shimadzu, IRAffinity-1S). The samples were prepared with the geopolymer mortar ground and sieved in 325 mesh. The spectra in the mid-infrared range were measured (400-4000 cm-1).
RESULTS AND DISCUSSION
For the preparation of the geopolymer, metakaolin was used as a source of aluminum and silicon; to prepare the activating solution, sodium silicate and sodium hydroxide were used. During the production process, it was observed that the increase in sodium silicate decreases the viscosity of the paste, changing the conformation conditions of specimens, this fact can be justified by the higher viscosity of sodium silicate about to sodium hydroxide 29),(30. The change in the proportions of the factors SiO2/Al2O3, Na2O/SiO2, and H2O/Na2O resulted in changes in the microstructure of the materials and the mechanical resistance.
The specimens have a rigid structure after 24 hours of curing at room temperature, just as Rovnaník 31. These specimens were cured for 7 days to perform the compressive strength test, the result shown in Figure 2 and Table 2 is the average obtained from 3 specimens. The compressive strength results allow us to analyze that by fixing the molarity of NaOH, the compressive strength increases with the addition of Na2SiO3 up to 7.5 Mols/L of NaOH. After this molarity, the behavior changes with the different quantities of sodium silicate, with less amount, the compressive strength increases, and in greater amount, the compressive strength decreases. According to Jaya et al., the increase in the concentration of NaOH facilitates the aluminosilicate dissolution process and the progress of geopolymerization. However, it does not increase the compressive strength after a certain concentration of NaOH 32.
This behavior presented in Figure 2 is indicative of the interaction between the variables considered in the study. In the graph shown in Figure 3, it is noted that increasing the Na2SiO3/NaOH ratio causes the average compression strength to increase gradually, the introduction of sodium silicate into the mixture results in strength gain in initial ages. In specimens with 10 moles/L of NaOH, the compressive strength decreases at a certain proportion of Na2SiO3/NaOH, so it is assumed that high NaOH molarity associated with high Na2SiO3/NaOH ratios results in decreased compressive strength.
For the three-dimensional polymeric structure of the geopolymers to be formed, there is a need for the reacted materials to have a proportional quantity to the tetrahedron network. Specimens with low sodium content have insufficient amounts of OH- to completely dissolve Si4+ and Al3+ from metakaolin, and Na+ is insufficient to allow complete polymerization of the network. Thus, unreacted metakaolin causes less strength 33. In specimens with a high sodium content, the excess of OH- allows the complete dissolution of Si4+ and Al3+ from metakaolin. However, the excess of sodium weakens the structure 33.
Results presented by Görhan and Kürklü 26 showed similar performance for materials prepared considering NaOH solutions with a concentration of 3, 6, and 9 Mols/L. In this study, it was considered Na2SiO3/NaOH mass ratio of 2.00, with fly ash and sand as precursors. It has been shown that increasing the molar concentration of the NaOH solution results in increased strength, but the excess can impair performance due to the excess of sodium in the structure.
Some authors explain that when NaOH and sodium silicate are used together as activators, their functions complement each other. This statement corresponds to most of the results obtained in this work. However, it is important to respect some proportions so that there is no saturation 14.
Figure 4 shows the results obtained in FTIR analysis of metakaolin-based geopolymers with different amounts of SiO2/Al2O3, Na2O/SiO2, and H2O/Na2O. This figure shows the spectra with a length between 400 and 4000 cm-1. In general, the interpretation of the vibrational spectra of silicates is very complex 28, but it is also very important in assigning the vibrations of the bands.
The band at 469 cm-1 is observed in all geopolymer samples, and it is related to the Si-O bending vibration 34. The bands at 1010 to 1021 cm-1 are assigned for asymmetric stretching vibrations of Si-O-T (T = tetrahedral Si or Al) in the geopolymer network and change substantially both in shape and intensity as a function of the molar ratio of SiO2 to Na2O in the activator 22),(28),(34)-(38. In Figure 4, it can be seen that these bands are related to the compressive strength obtained, Mix A showed the least compressive strength and also the lowest band, while Mix C has the highest compressive strength and also the largest band.
The adsorption band at 1400 and 1500 cm-1 is related to the stretching vibrations of the C-O bond of carbonate in sodium carbonates formed by the reaction of NaOH with atmospheric CO222),(38)-(40. The Na2CO3 is formed by the reaction of CO2 with mobile alkalis. This occurs predominantly at an early age due to the low reaction degree 40. These bands are inversely proportional to the SiO2/Al2O3 factor, oxygen joined with carbon dioxide and produced the stretching vibrations of the C - O bond. Mix A and Mix G have the lowest SiO2/Al2O3 rates in this group of samples and the largest adsorption bands.
The diffuse bands between 1700 and 3700cm-1 in the geopolymer samples are generally attributed to the presence of hydrated compounds with constitutional water tightly bound to the molecular structure 40. These bands are associated with the stretching and deformation vibrations of the physically adsorbed water molecules at the surface 28),(34. The presence of a wide band in the range 3700 cm-1 is due to the stretching vibrations of OH- groups. The range 1700 cm-1 is about bending vibrations of HOH groups. These bands confirm the presence of hydrated aluminosilicates in the resulting samples 22),(38. Thus, as these bands are related to the presence of compounds hydrated with water, it is noticed that the bands with higher values are also from mixtures with less compressive strength, suggesting that excess water in the structure causes a loss of mechanical strength.
The XRD patterns of the geopolymers produced are shown in Figure 5. In the metakaolin standard XRD shown in Figure 1, it can be seen that the amorphous structure is shown in the range from 15º to 25º (2θ). In the geopolymer patterns, the hump referring to the structure amorphous metakaolin is in the range from 20º to 35º (2θ) 17),(22),(41, suggesting that quartz did not participate in the geopolymerization reaction 41. The presence of the amorphous phase, indicated by the hump, is the sodium-aluminum-silicate-hydrate gel, the atmospheric carbon dioxide reacts with the alkaline activator resulting in the generation of sodium carbonates 22. However, the most striking feature of geopolymers is that, regardless of the choice of aluminosilicate source, activating solution, and curing condition, the large hump is present in all cases 17. In other words, the ubiquitous peak must be considered as the distinguishing characteristic of the diffractogram of any geopolymer, and therefore, its identification becomes central in determining the microstructure of a geopolymer 17.
The crystalline phases identified in the diffractogram quartz (SiO2, PDF No. 01-079-1910), muscovite (H2KAl3SiO12, PDF No. 00-007-0032) 17 and kaolinite (Al2Si2O5 (OH)4, PDF No. 01- 075-0938), that are, the remaining phases of the metakaolin that did not react during the geopolymerization process. However, no characteristic crystalline phase of this material is identified in the XRD analysis of geopolymeric products because the crystallinity observed in electron diffraction experiments is present in a length scale below the XRD detection limit 17.
In the diffractogram shown in Figure 5, the crystalline peaks have greater intensity in samples with lower NaOH content, and the peaks of the phases of mixtures A and C are more intense than in mixtures G and I. The excess of NaOH in the geopolymeric mixture significantly reduces the amount of the crystalline phase and changes its composition, the reduction of the crystallinity of materials with high levels of NaOH is due to the fast formation of a large number of nuclei, which bothers their growth into crystals 14. Crystallization is also considerably suppressed by the addition of sodium silicate, although there is no reaction with the use of sodium silicate alone, its presence, even in small amounts combined with NaOH, is effective in changing the crystallization mechanism 17.
The microstructure was analyzed using a scanning electron microscope (SEM) and a transmission electron microscope (TEM). Figure 6 shows SEM images of the produced geopolymers. Figure 6a indicates the presence of pores and cracks of different sizes on the surface of the material.
The interface between the binder and some pores has a layered texture. This effect occurs by removing the particles from the plate structure in the metakaolin during polishing 42, as in Figure 6b. The pore cross-sectional area caused by particle peeling indicates that the amount of material that did not react in the specimens after curing is significant. The metakaolin-based geopolymers form an amorphous substance with a lamellar structure. There are some metakaolin particles that did not react, looking like a loose structure, and the gel phase, which is tightly coupled, retracts during moisture loss, generating increased tensions and creating cracks 43), (44.
The geopolymers are formed by a long and resistant chain of particles called a geopolymer matrix or gel phase, observed with large magnifications, as shown in Figure 6c. The presence of nanometric pores can also be seen, which shows that the pores are part of the matrix.
The microstructures shown in Figure 7 reveal a uniform matrix, which appears to be a denser and firmer region, with the presence of dispersed particles, where similar micrographs were obtained by Kljajević et al.28, It is noted that these particles are loose in the geopolymer structure are materials that have not reacted and do not appear to be firmly adhered to the binder 42. In the SEM image in Figure 7, the loose structures are indicated by “1”, and the denser structures, where there is the gel phase with cracks originating during curing, are indicated by “2”. It can be seen in Figure 7 that the SiO2/Al2O3 ratio positively influences the microstructure of the material. A higher ratio used in the composition provides a material with fewer loose structures.
SEM images of the geopolymer indicating in “1” the gel phase and “2” the undissolved particles.
With the use of the material in nanometric dimensions, the high-resolution microscopy technique was used to observe the formation of the geopolymer phases 17. In Figure 8, TEM micrographs show images at a higher magnification than Figure 6c, corroborating that the geopolymeric material produced is formed by clusters of small particles with nanometric size wrapped in a nanoporosity region 16), (17.
TEM micrographs of the geopolymers of the extremes of the analyzed factors (a) Mix A, (b) Mix C, (c) Mix G, and (d) Mix H.
In the analyzed samples, the diffraction pattern of the amorphous and crystalline geopolymer gel was found, shown in Figure 9, the diffraction pattern with a cloudy ring represents the amorphous geopolymeric binding gel, and with dotted ring shape denotes the semi-crystalline/crystalline particles like quartz, mullite, etc 45.
The nanocrystalline regions in the circular particles observed under TEM provide electron diffraction patterns typical of crystalline structures, being sorted on a very short length scale to provide the X-ray diffractograms characteristic of their actual structure crystals. As the crystalline state minimizes the free energy of a system, the formation of crystalline regions through the process of dissolution-reprecipitation of geopolymerization is not unexpected 17.
CONCLUSION
In this study, nine mixtures were produced and cured at room temperature for 7 days to evaluate the microstructural effect and resistance to compression with the variation of the SiO2/Al2O3 and SiO2/Na2O ratios.
The increase in the Na2SiO3/NaOH ratio decreased the workability of the mixture once sodium silicate has a higher viscosity when compared to sodium hydroxide. The statistical analysis provided the best visualization of the effects that occur in the compressive strength, the Na2SiO3/NaOH ratio is the most important factor in the strength gain at early age. The increase in the molarity of NaOH does not significantly influence this property. The values obtained for compressive strength varied between 4.46 and 41.14 MPa as the smallest and highest SiO2/Al2O3 ratio, respectively.
The FTIR, XRD, and TEM techniques confirmed the amorphous structure formed by the geopolymer samples. The bands present in the FTIR are typical of this material, which suggests the process of geopolymerization. The main characteristic of XRD analysis is the presence of an amorphous hump between 20º and 35º (2θ), the crystalline phases identified are coming from the remaining phases of metakaolin that did not react.
In the microstructural analysis, the presence of the gel phase and particles that did not react during the geopolymerization process were identified. Cracks and pores were observed on the material surface. Larger magnifications show that geopolymers are clusters of nanometric particles in regions of nanoporosity.
These characteristics mentioned are related to SiO2/Al2O3 and SiO2/Na2O ratio variation in the geopolymerization. The results showed that it is possible to obtain a geopolymeric paste of metakaolin and sodium-based alkaline solution as an activating agent. Metakaolin must not present variations in properties, as this is a difficult factor to control. Even so, metakaolin can be considered a good activator compared to others, such as fly slag and ash, which are waste and may have even greater variations in characteristics.
ACKNOWLEDGMENT
The authors are thankful for the Multi-User Facility infrastructure of the State University of Santa Catarina, Technological Sciences Center.
The authors also are grateful to the research funding agencies, CAPES and FAPESC (3/2023), for their financial support. This study was financed in part by the Coordenação de Aperfeiçoamento de Pessoal de Nível Superior - Brasil (CAPES) - Finance Code 001.
REFERENCES
-
1 Torres-Carrasco M, Puertas F. Alkaline Activation of Different Aluminosilicates as an Alternative to Portland Cement: Alkali Activated Cements or Geopolymers. Rev Ing Constr. 32(2); 2017:5-12. doi:10.4067/S0718-50732017000200001.
» https://doi.org/10.4067/S0718-50732017000200001 -
2 Davidovits J. GEOPOLYMERS: Man-Made Rock Geosynthesis and the Resulting Development of Very Early High Strength Cement. Mater Educ. 16; 1994:1-25. doi:10.1016/0008-8846(94)00121-e.
» https://doi.org/10.1016/0008-8846(94)00121-e -
3 Borges PHR, Lourenço TMF, Foureaux AFS, Pacheco LS. Estudo comparativo da análise de ciclo de vida de concretos geopoliméricos e de concretos à base de cimento Portland composto (CP II). Ambient Constr. 14(2); 2014:153-68. doi:10.1590/S1678-86212014000200011.
» https://doi.org/10.1590/S1678-86212014000200011 -
4 Davidovits J. Geopolymers - Inorganic polymeric new materials. J Therm Anal. 37; 1991:1633-56. doi:10.1007/BF01912193.
» https://doi.org/10.1007/BF01912193 -
5 Petlitckaia S, Poulesquen A. Design of lightweight metakaolin based geopolymer foamed with hydrogen peroxide. Ceram Int. 45(1); 2019:1322-30. doi:10.1016/j.ceramint.2018.10.021.
» https://doi.org/10.1016/j.ceramint.2018.10.021 -
6 Songpiriyakij S, Kubprasit T, Jaturapitakkul C, Chindaprasirt P. Compressive strength and degree of reaction of biomass- and fly ash-based geopolymer. Constr Build Mater. 24(3); 2010:236-40. doi:10.1016/j.conbuildmat.2009.09.002.
» https://doi.org/10.1016/j.conbuildmat.2009.09.002 - 7 Pinto AT. Introdução ao estudo dos geopolímeros. Univ Trás-Os-Montes Alto Douro; 2006.
-
8 Lahoti M, Narang P, Tan KH, Yang E. Mix design factors and strength prediction of metakaolin-based geopolymer. Ceram Int . 43(14); 2017:11433-41. doi:10.1016/j.ceramint.2017.06.006.
» https://doi.org/10.1016/j.ceramint.2017.06.006 -
9 Vafaei M, Allahverdi A. Durability of Geopolymer Mortar Based on Waste-Glass Powder and Calcium Aluminate Cement in Acid Solutions. J Mater Civ Eng. 29(10); 2017:04017196. doi:10.1061/(asce)mt.1943-5533.0002053.
» https://doi.org/10.1061/(asce)mt.1943-5533.0002053 -
10 Li Z, Zhang S, Zuo Y, Chen W, Ye G. Chemical deformation of metakaolin based geopolymer. Cem Concr Res. 120; 2019:108-18. doi:10.1016/j.cemconres.2019.03.017.
» https://doi.org/10.1016/j.cemconres.2019.03.017 -
11 Sani NAM, Man Z, Shamsuddin RM, Azizli KA, Shaari KZK. Determination of Excess Sodium Hydroxide in Geopolymer by Volumetric Analysis. Procedia Eng. 148; 2016:298-301. doi:10.1016/j.proeng.2016.06.621.
» https://doi.org/10.1016/j.proeng.2016.06.621 -
12 Ali AA, Al-Attar TS, Abbas WA. Mechanical Performance of Blended Fly Ash-based Geopolymer Concrete with GGBS and Metakaolin. Eng Technol J. 40; 2022:819-31. doi:10.30684/ETJ.2022.132647.1135.
» https://doi.org/10.30684/ETJ.2022.132647.1135 -
13 Palomo A, Blanco-Varela MT, Granizo ML, Puertas F, Vazquez T, Grutzeck MW. Chemical stability of cementitious materials based on metakaolin. Cem Concr Res . 29(7); 1999:997-1004. doi:10.1016/S0008-8846(99)00074-5.
» https://doi.org/10.1016/S0008-8846(99)00074-5 -
14 Zhang B, MacKenzie KJD, Brown IWM. Crystalline phase formation in metakaolinite geopolymers activated with NaOH and sodium silicate. J Mater Sci. 44; 2009:4668-76. doi:10.1007/s10853-009-3715-1.
» https://doi.org/10.1007/s10853-009-3715-1 -
15 Kara I, Tunc D, Sayin F, Akar ST. Study on the performance of metakaolin based geopolymer for Mn(II) and Co(II) removal. Appl Clay Sci. 161; 2018:184-93. doi:10.1016/j.clay.2018.04.027.
» https://doi.org/10.1016/j.clay.2018.04.027 -
16 Maitland CF, Buckley CE, O’Connor BH, Butler PD, Hart RD. Characterization of the pore structure of metakaolin-derived geopolymers by neutron scattering and electron microscopy. J Appl Crystallogr. 44; 2011:697-707. doi:10.1107/S0021889811021078.
» https://doi.org/10.1107/S0021889811021078 -
17 Provis JL, Lukey GC, Van Deventer JSJ. Do geopolymers actually contain nanocrystalline zeolites? A reexamination of existing results. Chem Mater. 17(12); 2005:3075-85. doi:10.1021/cm050230i.
» https://doi.org/10.1021/cm050230i - 18 Hardjito D, Rangan BV. Development and properties of low-calcium fly ash-based geopolymer concrete. Res Rep GC. 94; 2005.
-
19 Ghanbari M, Hadian AM, Nourbakhsh AA, MacKenzie KJD. Modeling and optimization of compressive strength and bulk density of metakaolin-based geopolymer using central composite design: A numerical and experimental study. Ceram Int . 43(1A); 2017:324-35. doi:10.1016/j.ceramint.2016.09.159.
» https://doi.org/10.1016/j.ceramint.2016.09.159 -
20 Ali AA, Al-Attar TS, Abbas WA. A statistical model to predict the strength development of geopolymer concrete based on SiO2/Al2O3 ratio variation. Civ Eng J. 8(3); 2022:454-71. doi:10.28991/CEJ-2022-08-03-04.
» https://doi.org/10.28991/CEJ-2022-08-03-04 -
21 Ali AA, Al-Attar TS, Abbas WA. A statistical models to predict strength development of eight molarity geopolymer concrete. Case Stud Constr Mater. 17; 2022:e01304. doi:10.1016/J.CSCM.2022.E01304.
» https://doi.org/10.1016/J.CSCM.2022.E01304 -
22 Brylewska K, Rożek P, Król M, Mozgawa W. The influence of dealumination/desilication on structural properties of metakaolin-based geopolymers. Ceram Int . 44(11); 2018:12853-61. doi:10.1016/j.ceramint.2018.04.095.
» https://doi.org/10.1016/j.ceramint.2018.04.095 -
23 Subaer S, Van Riessen A. Thermo-mechanical and microstructural characterisation of sodium-poly(sialate-siloxo) (Na-PSS) geopolymers. J Mater Sci . 42; 2007:3117-23. doi:10.1007/s10853-006-0522-9.
» https://doi.org/10.1007/s10853-006-0522-9 -
24 Raj S, Sharma AK, Anand KB. Performance appraisal of coal ash stabilized rammed earth. J Build Eng. 18; 2018:51-7. doi:10.1016/j.jobe.2018.03.001.
» https://doi.org/10.1016/j.jobe.2018.03.001 - 25 Kriven WM, Bell JL, Gordon M. Microstructure and microchemistry of fully-reacted geopolymers and geopolymer matrix composites. Adv Ceram Matrix Compos IX. 227-50; 2004. doi:10.1002/9781118406892.ch15.
-
26 Görhan G, Kürklü G. The influence of the NaOH solution on the properties of the fly ash-based geopolymer mortar cured at different temperatures. Compos B Eng. 58; 2014:371-7. doi:10.1016/J.COMPOSITESB.2013.10.082.
» https://doi.org/10.1016/J.COMPOSITESB.2013.10.082 -
27 ABNT. NBR 7215 - Portland cement - Determination of compressive strength of cylindrical test specimens. Brazilian Association for Technical Standards; 2019. doi:10.1520/c0039_c0039m-15a.
» https://doi.org/10.1520/c0039_c0039m-15a -
28 Kljajević LM, Nenadović SS, Nenadović MT, Bundaleski NK, Todorović B, Pavlović VB, Rakočević ZL. Structural and chemical properties of thermally treated geopolymer samples. Ceram Int . 43(9); 2017:6700-8. doi:10.1016/j.ceramint.2017.02.066.
» https://doi.org/10.1016/j.ceramint.2017.02.066 -
29 Sathonsaowaphak A, Chindaprasirt P, Pimraksa K. Workability and strength of lignite bottom ash geopolymer mortar. J Hazard Mater. 168(1); 2009:44-50. doi:10.1016/j.jhazmat.2009.01.120.
» https://doi.org/10.1016/j.jhazmat.2009.01.120 -
30 Chindaprasirt P, Chareerat T, Sirivivatnanon V. Workability and strength of coarse high calcium fly ash geopolymer. Cem Concr Comp. 29(3); 2007:224-9. doi:10.1016/j.cemconcomp.2006.11.002.
» https://doi.org/10.1016/j.cemconcomp.2006.11.002 -
31 Rovnaník P. Effect of curing temperature on the development of hard structure of metakaolin-based geopolymer. Constr Build Mater . 24(7); 2010:1176-83. doi:10.1016/j.conbuildmat.2009.12.023.
» https://doi.org/10.1016/j.conbuildmat.2009.12.023 -
32 Jaya NA, Yun-Ming L, Cheng-Yong H, Abdullah MMAB, Hussin K. Correlation between pore structure, compressive strength and thermal conductivity of porous metakaolin geopolymer. Constr Build Mater . 247; 2020:118641. doi:10.1016/j.conbuildmat.2020.118641.
» https://doi.org/10.1016/j.conbuildmat.2020.118641 -
33 Rowles M, O’Connor B. Chemical optimisation of the compressive strength of aluminosilicate geopolymers synthesised by sodium silicate activation of metakaolinite. J Mater Chem. 13; 2003:1161-5. doi:10.1039/b212629j.
» https://doi.org/10.1039/b212629j -
34 Aredes FGM, Campos TMB, Machado JPB, Sakane KK, Thim GP, Brunelli DD. Effect of cure temperature on the formation of metakaolinite-based geopolymer. Ceram Int . 41(6); 2015:7302-11. doi:10.1016/j.ceramint.2015.02.022.
» https://doi.org/10.1016/j.ceramint.2015.02.022 -
35 Zhang Z, Provis JL, Wang H, Bullen F, Reid A. Quantitative kinetic and structural analysis of geopolymers. Part 2. Thermodynamics of sodium silicate activation of metakaolin. Thermochim Acta. 565; 2013:163-71. doi:10.1016/j.tca.2013.01.040.
» https://doi.org/10.1016/j.tca.2013.01.040 -
36 Chen X, Niu Z, Wang J, Zhu GR, Zhou M. Effect of sodium polyacrylate on mechanical properties and microstructure of metakaolin-based geopolymer with different SiO3/Al2O3 ratio. Ceram Int . 44(15); 2018:18173-80. doi:10.1016/j.ceramint.2018.07.025.
» https://doi.org/10.1016/j.ceramint.2018.07.025 -
37 Torres-Carrasco M, Puertas F. Waste glass in the geopolymer preparation. Mechanical and microstructural characterization. J Clean Prod. 90; 2015:397-408. doi:10.1016/j.jclepro.2014.11.074.
» https://doi.org/10.1016/j.jclepro.2014.11.074 -
38 Król M, Minkiewicz J, Mozgawa W. IR spectroscopy studies of zeolites in geopolymeric materials derived from kaolinite. J Mol Struct. 1126; 2016:200-6. doi:10.1016/j.molstruc.2016.02.027.
» https://doi.org/10.1016/j.molstruc.2016.02.027 -
39 Rovnaník P, Rovnaníková P, Vyšvar M, Grzeszczyk S, Janowska-Renkas E. Rheological properties and microstructure of binary waste red brick powder/metakaolin geopolymer. Constr Build Mater . 188; 2018:924-33. doi:10.1016/j.conbuildmat.2018.08.150.
» https://doi.org/10.1016/j.conbuildmat.2018.08.150 -
40 Sun Z, Vollpracht A. One year geopolymerisation of sodium silicate activated fly ash and metakaolin geopolymers. Cem Concr Comp . 95; 2019:98-110. doi:10.1016/j.cemconcomp.2018.10.014.
» https://doi.org/10.1016/j.cemconcomp.2018.10.014 -
41 Chen L, Wang Z, Wang Y, Feng J. Preparation and properties of alkali activated metakaolin-based geopolymer. Materials. 9; 2016:1-12. doi:10.3390/ma9090767.
» https://doi.org/10.3390/ma9090767 -
42 Duxson P, Provis JL, Lukey GC, Mallicoat SW, Kriven WM, Van Deventer JSJ. Understanding the relationship between geopolymer composition, microstructure and mechanical properties. Colloids Surf A Physicochem Eng Asp. 269(1-3); 2005:47-58. doi:10.1016/j.colsurfa.2005.06.060.
» https://doi.org/10.1016/j.colsurfa.2005.06.060 -
43 Li W, Lemougna PN, Wang K, He Y, Tong Z, Cui X. Effect of vacuum dehydration on gel structure and properties of metakaolin-based geopolymers. Ceram Int . 43(16); 2017:14340-6. doi:10.1016/j.ceramint.2017.07.190.
» https://doi.org/10.1016/j.ceramint.2017.07.190 -
44 Kong DLY, Sanjayan JG. Effect of elevated temperatures on geopolymer paste, mortar and concrete. Cem Concr Res . 40(2); 2010:334-9. doi:10.1016/j.cemconres.2009.10.017.
» https://doi.org/10.1016/j.cemconres.2009.10.017 -
45 Revathi T, Jeyalakshmi R, Rajamane NP. Micro-Structural Characterization of Activating Solution with Siliceous Species on Chemical Reactivity of Geopolymer by Advanced Analytical Techniques. Asian J Chem. 30(11); 2018:2404-10. doi:10.14233/AJCHEM.2018.21415.
» https://doi.org/10.14233/AJCHEM.2018.21415