Open-access Optimizing high strength concrete: a comprehensive study on the synergistic effects of natural fibres and silica fume on workability, mechanical and flexural behavior

ABSTRACT

This research explores the synergistic effects of natural fiber reinforcement, specifically manila hemp, and silica fume incorporation on the performance of high-strength concrete (HSC). Various concrete mixtures were developed with different proportions of natural fibers (0%, 0.5%, 1.0%, 1.5%, and 2.0% by volume) and silica fume (0% to 30% by increment of 5% in weight of cement). A series of tests were conducted to evaluate workability, mechanical properties (including compressive, tensile, and flexural strength), and flexural aspects (such as deflection of beam). The findings demonstrate that incorporating up to 1.5% natural fibers and silica fume content up to 20% was found to improve mechanical property of 21% and flexural property of 18% due to its pozzolanic properties and ability to optimize particle packing. However, increasing the fiber and silica fume content beyond these levels resulted in reduced workability and only minimal improvements in strength. The study identified an optimal mixture consisting of 1.0% natural fibers and 20% silica fume, achieving a balance between improved mechanical properties, enhanced flexural behavior, and acceptable workability. This combined approach provides a promising strategy for developing high-strength concrete with advanced performance.

Keywords:
Natural fibre; Manila hemp; Silica fume; Mechanical property; Flexural behavior

1. INTRODUCTION

In composite materials, natural fibers have drawn a lot of interest lately as ecological substitutes for synthetic fibers. Abaca, or manila hemp, is one of them and has showed promise because of its endurance and strong tensile strength. It has been investigated if silica fume can improve the mechanical and durability qualities of composite materials. With an emphasis on manila hemp and the function of silica fume, this literature review attempts to present a thorough summary of the most recent findings on the mechanical characteristics and flexural behavior of natural fiber composites.

The potential of natural fibers like flax, kenaf, and hemp to reinforce polymer matrices has been thoroughly investigated. A few examples of the variables that affect these composites’ mechanical characteristics include surface treatment, fiber alignment, and content [1]. Hemp and kenaf fiber composites’ mechanical characteristics are greatly enhanced by alkalization and fiber alignment [2]. Alkalized long kenaf-polyester composites, for instance, exhibit superior mechanical properties compared to their hemp counterparts. The removal of surface impurities through alkalization enhances the flexural modulus and strength of the composites [3]. Comparative studies between epoxy and polyester matrices reinforced with hemp fibers indicate that epoxy composites generally exhibit superior mechanical properties. For instance, epoxy composites with 30% hemp fiber content show higher flexural and tensile strength compared to polyester composites. This suggests that epoxy is a more suitable matrix for high-performance applications [4].

The combination of different natural fibers, such as hemp and nettle, in a polyester resin matrix has been explored to achieve high mechanical properties. These hybrid composites demonstrate improved hardness, tensile, flexural, and impact resistance, making them suitable for various applications [5]. The incorporation of hemp fibers into thermoplastic polyurethane (TPU) matrices has also been investigated. Increasing the fiber volume content enhances the flexural strength of the composites [6]. The optimum fiber length and surface treatment further improve the mechanical properties, indicating the potential of hemp-TPU composites in balancing flexural and tensile properties [7].

The alignment and volume content of fibers play a vital role in determining the flexural behavior of natural fiber composites. Alkalized and aligned fibers generally result in higher flexural modulus and strength. For example, alkalized long kenaf-CNSL composites exhibit superior flexural properties compared to random fiber composites [8]. The viscoelastic behavior of natural fiber composites, including their storage modulus and damping factor, has been studied using dynamic mechanical analysis [9]. The addition of fillers such as barium sulfate can enhance the loss modulus, indicating improved energy dissipation capabilities. However, the tensile strength may be adversely affected by the addition of such fillers [10]. The incorporation of silica fume and other mineral admixtures in fiber-reinforced concrete (FRC) significantly influences its flexural behavior and durability [11]. Concrete’s endurance is improved by silica fume in particular, and its toughness and post-cracking flexural resistance are enhanced when fibers are added. Combining several fiber types, including steel and polyvinyl alcohol (PVA) fibers, might enhance hybrid fiber reinforced composites’ flexural performance even further [12].

As a byproduct of the manufacture of silicon and ferrosilicon alloys, silica fume is commonly employed in concrete as a pozzolanic ingredient. Its addition can improve the mechanical and lasting qualities of composites made of natural fibers [13, 14]. Fiber-reinforced concrete is made more durable by adding silica fume, which increases electrical resistivity and decreases chloride diffusivity. As a result, the concrete becomes higher-performing and more resilient, making it appropriate for structural uses [15, 16]. Through strengthening the connection between the fibers and the matrix, silica fume improves the flexural performance of composite materials. The composites are therefore more suited for load-bearing applications because to their increased flexural strength and modulus [17, 18].

The research on natural fiber composites, particularly those reinforced with manila hemp and enhanced with silica fume, demonstrates significant potential for various industrial applications. The mechanical properties and flexural behavior of these composites are influenced by factors such as fiber content, alignment, surface treatment, and the incorporation of mineral admixtures. Research gaps on optimizing these parameters to develop high-performance, sustainable composite materials for structural applications.

2. MATERIAL AND METHODS

2.1. Cement

The material used in this study exhibits the following properties: a relative density of 3.15 and standard consistency of 29.12%. Its initial and final setting times are 34 minutes and 4 hours 41 minutes, respectively [19]. The soundness test, conducted using Le-Chatelier’s apparatus, indicated a value of 0.99 mm, while the 28-day compressive strength reached 53.42 MPa. The chemical composition includes 20.99% silica (SiO2), 6.05% alumina (Al2O3), 6.01% ferric oxide (Fe2O3), 62.74% calcium oxide (CaO), 1.33% magnesium oxide (MgO), 1.82% sulfuric anhydride (SO3), and 1.14% loss on ignition (LOI). Additionally, the material contains 0.8% alkalies, 0.015% chlorides, and a lime saturation factor (LSF) of 0.88%. Table 1 shows the properties of cement.

Table 1
Properties of cement.

2.2. Coarse aggregate

Table 2 provides the physical properties of the coarse aggregate used in the study. The relative density of the aggregate is 2.78, indicating its relative density. The fineness modulus of 6.17 suggests the aggregate’s particle size distribution is within a coarse range. With a percentage voids value of 37.04%, the aggregate exhibits significant porosity [20]. The crushing value of 23.74% reflects the aggregate’s strength and resistance to crushing. Water absorption is low at 0.5%, indicating minimal porosity. The aggregate is dark grey in color and has an angular shape, contributing to good interlocking in the concrete matrix.

Table 2
Physical properties of coarse aggregate.

2.3. Fine aggregate

Table 3 outlines the physical properties of the fine aggregate utilized in the research. The relative density is 2.63, which suggests the relative density of the material [21]. With a fineness modulus of 2.67, the aggregate is within the ideal range for fine materials, indicating an appropriate particle size distribution. The bulk density is recorded at 1676 kg/m3, providing insight into the material’s compactness. The free moisture content is low at 0.11%, signifying minimal retained moisture, while the water absorption rate of 0.74% reflects the aggregate’s ability to retain water, which can impact the concrete’s overall performance.

Table 3
Physical properties of fine aggregate.

2.4. Silica fume

Table 4 presents the mechanical properties of the silica fume used in the study. The relative density is 2.64, indicating a density similar to that of the fine aggregate [22]. The fineness modulus of 2.1 highlights its fine particle size, which can enhance the microstructure of the concrete. With a water absorption rate of 0.25%, the silica fume has low porosity, contributing to its effective use as a pozzolanic material. The material is white in color and has a bulk density of 240 kg/m3, reflecting its lightweight nature. The free moisture content is minimal at 0.05%, indicating very low retained moisture.

Table 4
Physical properties of silica fume.

2.5. Manila hemp

Table 5 details the physical properties of Manila hemp utilized in the study. The material has a density of 1.4 g/cc, making it relatively lightweight. Its tensile strength is 650 MPa, indicating robust fiber quality, while the elastic modulus of 721 GPa signifies high stiffness [23]. The specific strength of 584 s/g and specific modulus of 50 demonstrate the material’s favorable strength-to-weight and stiffness-to-weight ratios, respectively. Additionally, the moisture content of 9.5% indicates the fiber’s ability to retain a moderate amount of water, which could influence its behavior in composite materials.

Table 5
Physical properties of manila hemp.

2.6. Super plasticizer

Table 6 outlines the mechanical properties of the superplasticizer used in the study. The material is a beige liquid with a specific gravity of 1.11, indicating its density relative to water. It is chemically composed of polycarboxylate ether, with 41% active ingredients, enhancing its effectiveness in improving the workability of concrete [24]. The pH value ranges from 7 to 8, ensuring a neutral to slightly alkaline solution, which is suitable for concrete applications. Importantly, the superplasticizer is chloride-free, making it safe for use in reinforced concrete structures by preventing potential corrosion of the steel reinforcement. Figure 1 shows the materials used in this research.

Table 6
Physical properties of super plasticizer.
Figure 1
Shows the materials used in this research.

3. METHODOLOGY

The methodology for producing high-strength concrete M60 involves using OPC 53, fine aggregate, silica fume, Manila hemp fibers, and a polycarboxylate ether-based superplasticizer. The mix design is tailored to achieve a water-cement ratio of 0.30, incorporating silica fume as 0–30% of cement by weight and Manila hemp fibers at 0%–1.5%. The dry materials are first mixed, followed by the gradual addition of fibers to ensure even distribution [25, 26]. The wet mixing process includes adding water mixed with the superplasticizer to achieve the desired workability [27]. The concrete is then cast, compacted, cured, and tested for mechanical property and flexural properties [28].

4. RESULTS AND DISCUSSION

4.1. Slump cone test

The results indicate the impact of varying proportions of silica fume and Manila hemp fibers on the slump values of concrete mixes. The conventional concrete mix (M1) achieved the highest slump value of 81 mm, indicating better workability. As silica fume content increases from 5% to 30% (M2–M7), the slump values slightly decrease, showing a minor reduction in workability due to the finer particles of silica fume, which increase the mix’s viscosity. When Manila hemp fibers are added (M8–M15), a more noticeable decline in slump values is observed, particularly with higher fiber content. For example, M8 with 0.5% Manila hemp and 20% silica fume has a slump of 70 mm, while M15 with 2% Manila hemp and 25% silica fume has a slump of 61 mm. This reduction suggests that the addition of fibers leads to increased internal friction within the mix, reducing flowability. The combination of silica fume and Manila hemp fibers enhances the concrete’s strength and durability but compromises workability. The results highlight the need for careful optimization of fiber content to maintain an acceptable balance between workability and the desired mechanical properties in high-performance concrete mixes. Figure 2 shows the test results of slump cone test.

Figure 2
Slump cone test.

4.2. Compaction factor test

The results show the compaction factor for various concrete mixes incorporating different proportions of silica fume and Manila hemp fibers. The conventional concrete (M1) exhibits the highest compaction factor of 0.846, indicating excellent workability. As silica fume content increases from 5% to 30% (M2–M7), the compaction factor generally decreases, reflecting a slight reduction in the ease of compaction due to the finer particles of silica fume, which increase the mix’s cohesiveness. When Manila hemp fibers are added (M8–M15), the compaction factor further declines, particularly with higher fiber content. For instance, M8 with 0.5% Manila hemp and 20% silica fume has a compaction factor of 0.732, while M15 with 2% Manila hemp and 25% silica fume has the lowest compaction factor of 0.637. This reduction suggests that the inclusion of fibers increases the internal resistance to compaction, reducing the mix’s flowability and ease of compaction. While the incorporation of silica fume and Manila hemp fibers enhances the mechanical properties and durability of the concrete, it compromises the compaction factor, indicating reduced workability. These results underscore the importance of optimizing the mix design to achieve a balance between workability and the desired performance characteristics in high-strength concrete. Figure 3 shows the compaction factor test.

Figure 3
Compaction factor test.

4.3. Compressive strength test

Conventional concrete (M1) exhibited a steady increase in strength from 43.88 MPa at 7 days to 68.91 MPa at 90 days. The addition of silica fume consistently enhanced the strength across all curing periods, with mixes M2 to M6 showing improved results compared to the conventional mix. Specifically, M6, with 25% silica fume and 75% OPC, achieved the highest strength values, reaching 75.69 MPa at 90 days. The inclusion of Manila hemp fibers in concrete mixes (M8 to M15) generally led to a reduction in compressive strength compared to the corresponding mixes without hemp. For instance, M8, which includes 20% silica fume, 75% OPC, and 0.5% Manila hemp, showed lower strengths than M5 and M6, although it still performed better than mixes with higher hemp content (M9 to M15). As the percentage of Manila hemp increased, the compressive strength progressively decreased, with M15 showing the lowest strength of 65.97 MPa at 90 days. While silica fume significantly enhances the compressive strength of concrete, the addition of Manila hemp appears to compromise this benefit. Future work should explore optimizing the balance between silica fume and Manila hemp to achieve desired mechanical properties. Figure 4 shows the compressive strength test results.

Figure 4
Compressive strength test results.

4.4. Split tensile strength

Conventional concrete (M1) demonstrated a gradual enrichment in tensile strength from 3.59 MPa at 7 days to 4.22 MPa at 28 days. Incorporating silica fume generally improved tensile strength compared to the conventional mix. Among the silica fume mixes, M6, with 25% silica fume and 75% OPC, achieved the highest tensile strength, reaching 4.66 MPa at 28 days. The addition of Manila hemp fibers influenced the split tensile strength adversely. For example, M8, containing 20% silica fume, 75% OPC, and 0.5% Manila hemp, showed a lower tensile strength compared to M5, which had no hemp. As the Manila hemp content increased, the tensile strength decreased further, with M15 exhibiting the lowest strength of 4.04 MPa at 28 days. While silica fume enhances the split tensile strength of concrete, the incorporation of Manila hemp seems to diminish these benefits. The results suggest that balancing the proportions of silica fume and Manila hemp is crucial for optimizing the tensile properties of concrete. Figure 5 shows the split tensile strength test results.

Figure 5
Split tensile strength test results.

4.5. Flexural strength

The flexural strength test results are summarized in Table 3. Conventional concrete (M1) demonstrated an increase in flexural strength from 4.28 MPa at 7 days to 6.59 MPa at 28 days. Incorporating silica fume into the mix consistently improved flexural strength. Specifically, M6, with 25% silica fume and 75% OPC, achieved the highest flexural strength, reaching 7.28 MPa at 28 days. The inclusion of Manila hemp fibers had a variable effect on flexural strength. For instance, M8, which contains 20% silica fume, 75% OPC, and 0.5% Manila hemp, showed a slight decrease in strength compared to M5. However, mixes with higher amounts of Manila hemp, such as M10 and M15, exhibited only marginal reductions in strength compared to their counterparts without hemp. M15, with 25% silica fume, 75% OPC, and 2% Manila hemp, maintained a robust flexural strength of 6.90 MPa at 28 days. The silica fume significantly enhances the flexural strength of concrete, while the addition of Manila hemp has a minimal impact on this property. The results suggest that while silica fume effectively improves concrete performance, the addition of Manila hemp significantly improve its flexural strength. Figure 6 shows the flexural strength test results.

Figure 6
Flexural strength test results.

4.6. Flexural behavior of beam

The Figure 7, 8, 9 and 10 presents load-deflection data for four different concrete mixes: Conventional Concrete (M1), 25% Silica Fume + 75% OPC (M6), 20% Silica Fume + 75% OPC + 1.5% Manila Hemp (M10), and 25% Silica Fume + 75% OPC + 1.5% Manila Hemp (M14). The load (P) ranges from 0 kN to 125 kN, and the corresponding deflections (δ) are measured in millimeters for each mix. M1, the conventional concrete, exhibits the highest deflection under increasing load, especially beyond 65 kN, where it starts to diverge significantly from the other mixes. This indicates that M1 has the least stiffness among the tested mixes. In contrast, M14 consistently shows the lowest deflection across all load levels, demonstrating superior stiffness and load-bearing capacity. This improvement can be attributed to the combined effect of silica fume and Manila hemp fibers, which enhance the mix’s tensile strength and crack resistance. M6, with only silica fume added, and M10, with both silica fume and Manila hemp, perform better than M1 but not as well as M14. Notably, M10 shows slightly higher deflection than M6 at higher loads, suggesting that the inclusion of Manila hemp fibers at this composition may not provide as significant a reinforcement effect as in M14. The results indicate that the inclusion of both silica fume and Manila hemp fibers (M14) results in the most effective mix in terms of reducing deflection under load, thereby enhancing the concrete’s structural performance.

Figure 7
Deflection of M1 mix.
Figure 8
Deflection of M6 mix.
Figure 9
Deflection of M10 mix.
Figure 10
Deflection of M14 mix.

5. CONCLUSION

The experimental results reveal the impact of silica fume and Manila hemp fibers on the workability and physical properties of concrete. Conventional concrete (M1) achieved a slump value of 81 mm and a compaction factor of 0.846, demonstrating good workability. However, as the percentage of silica fume enriched and Manila hemp fibers were introduced, the slump values decreased, indicating a reduction in workability. For instance, Mix M14, which contains 25% silica fume and 1.5% Manila hemp, exhibited a slump value of 64 mm and a compaction factor of 0.669, the lowest among all mixes, signifying increased stiffness due to fiber addition.

In terms of compressive strength, silica fume significantly improved performance up to M6, which contained 25% silica fume, reaching 48.27 MPa at 7 days and 70.23 MPa at 28 days. However, the introduction of Manila hemp fibers in Mix M14 slightly reduced compressive strength, with M14 achieving 42.59 MPa at 7 days and 61.76 MPa at 28 days. Despite this reduction, the mixes with fibers still maintained respectable strength, indicating a balance between improved ductility and adequate compressive strength. The split tensile strength and flexural strength also followed a similar trend. Mix M6 exhibited the highest tensile and flexural strengths, with 4.66 MPa and 7.28 MPa at 28 days, respectively. Conversely, the addition of Manila hemp fibers in Mix M14 slightly reduced these values, with 4.12 MPa for split tensile strength and 6.95 MPa for flexural strength at 28 days. This reduction can be attributed to the fibrous nature of Manila hemp, which, while enhancing the toughness and crack resistance of the concrete, may slightly compromise strength metrics. The incorporation of silica fume enhances the strength and durability of concrete, while the addition of Manila hemp fibers improves toughness and crack resistance, although at the expense of some compressive and tensile strength.

M14, containing 25% silica fume and 1.5% Manila hemp, exhibited the lowest deflections across all load levels, indicating superior stiffness and load-bearing capacity. This mix outperformed others, demonstrating the effective reinforcement of silica fume and Manila hemp fibers in enhancing concrete’s structural performance.

6. BIBLIOGRAPHY

  • [1] AZIZ, S.H., ANSELL, M., “The effect of alkalization and fibre alignment on the mechanical and thermal properties of kenaf and hemp bast fibre composites: Part 1 – polyester resin matrix”, Composites Science and Technology, v. 64, n. 9, pp. 1219–1230, 2004. doi: http://doi.org/10.1016/j.compscitech.2003.10.001.
    » https://doi.org/10.1016/j.compscitech.2003.10.001
  • [2] AZIZ, S.H., ANSELL, M., “The effect of alkalization and fibre alignment on the mechanical and thermal properties of kenaf and hemp bast fibre composites: Part 2 – cashew nut shell liquid matrix”, Composites Science and Technology, v. 64, n. 9, pp. 1231–1238, 2004. doi: http://doi.org/10.1016/j.compscitech.2003.10.002.
    » https://doi.org/10.1016/j.compscitech.2003.10.002
  • [3] THIRUKUMARAN, T., KRISHNAPRIYA, S., PRIYA, V., et al, “Utilizing rice husk ash as a bio-waste material in geopolymer composites with aluminium oxide”, Global NEST Journal, v. 25, n. 6, pp. 119–129, 2023.
  • [4] NEVES, A.C.C., ROHEN, L.A., MANTOVANI, D.P., et al, “Comparative mechanical properties between biocomposites of Epoxy and polyester matrices reinforced by hemp fiber”, Journal of Materials Research and Technology, v. 9, n. 2, pp. 1296–1304, 2020. doi: http://doi.org/10.1016/j.jmrt.2019.11.056.
    » https://doi.org/10.1016/j.jmrt.2019.11.056
  • [5] PRASAD, L., ASHISH KUMAIN, R., PATEL, R.V., et al, “Physical and mechanical behavior of hemp and nettle fiber-reinforced polyester resin-based hybrid composites”, Journal of Natural Fibers, v. 19, n. 7, pp. 2632–2647, 2020. doi: http://doi.org/10.1080/15440478.2020.1821284.
    » https://doi.org/10.1080/15440478.2020.1821284
  • [6] VERAPATHRAN, M., VIVEK, S., ARUNKUMAR, G.E., et al, “Flexural behaviour of HPC beams with steel slag aggregate”, Journal of Ceramic Processing Research, v. 24, n. 1, pp. 89–97, 2023.
  • [7] CAMPOMORI, J.B., HUGEN, L.N., FLÁVIO DE ANDRADE, S., et al, “Effect of hot water and corona discharge treatments on the bonding behavior of jute fibers in polyester matrix”, Discover Materials, v. 4, n. 1, pp. 1–12, 2024. doi: http://doi.org/10.1007/s43939-024-00085-7.
    » https://doi.org/10.1007/s43939-024-00085-7
  • [8] ASYRAF, M.R.M., SHENG, D.D.C.V., MAS’OOD, N.N., et al, “Thermoplastic composites reinforced chemically modified kenaf fibre: current progress on mechanical and dynamic mechanical properties”, Biomass Conversion and Biorefinery, pp. 1–21, 2024. doi: http://doi.org/10.1007/s13399-024-05659-2.
    » https://doi.org/10.1007/s13399-024-05659-2
  • [9] ARASU, A., NATARAJAN, M., BALASUNDARAM, N., et al, “Utilizing recycled nanomaterials as a partial replacement for cement to create high-performance concrete”, Global NEST Journal, v. 25, n. 6, pp. 89–92, 2023.
  • [10] VARUTHAIYA, M., PALANISAMY, C., SIVAKUMAR, V., et al, “Concrete with sisal fibered geopolymer: a behavioral study”, Journal of Ceramic Processing Research, v. 23, n. 6, pp. 912–919, 2022.
  • [11] SAHU, S.B.B.P.J., NAYAK, S., SAHU, S., et al, “Extraction and characterization of natural CASCABELA thevetia bast fibers: a potential candidate as reinforcement in epoxy composites”, Journal of Natural Fibers, v. 20, n. 2, pp. 2272215, 2023. doi: http://doi.org/10.1080/15440478.2023.2272215.
    » https://doi.org/10.1080/15440478.2023.2272215
  • [12] WU, Z., KHAYAT, K., SHI, C., “Changes in rheology and mechanical properties of ultra-high performance concrete with silica fume content”, Cement and Concrete Research, v. 123, pp. 105786, 2019. doi: http://doi.org/10.1016/j.cemconres.2019.105786.
    » https://doi.org/10.1016/j.cemconres.2019.105786
  • [13] ARASU, A.N., MUTHUSAMY, N., NATARAJAN, B., et al, “Optimization of high performance concrete composites by using nano materials”, Research on Engineering Structures and Materials, v. 9, n. 3, pp. 843–859, 2023. doi: http://doi.org/10.17515/resm2022.602ma1213.
    » https://doi.org/10.17515/resm2022.602ma1213
  • [14] HAGHIGHATNIA, T., ABBASIAN, A., MORSHEDIAN, J., “Hemp fiber reinforced thermoplastic polyurethane composite: an investigation in mechanical properties”, Industrial Crops and Products, v. 108, pp. 853–863, 2017. doi: http://doi.org/10.1016/j.indcrop.2017.07.020.
    » https://doi.org/10.1016/j.indcrop.2017.07.020
  • [15] ARASU, A.N., NATARAJAN, M., BALASUNDARAM, N., et al, “Development of high-performance concrete by using nanomaterial graphene oxide in partial replacement for cement”, In: AIP Conference Proceedings, v. 2861, n. 1, 2023. doi: http://doi.org/10.1063/5.0158487.
    » https://doi.org/10.1063/5.0158487
  • [16] ALKBIR, M., SAPUAN, S., NURAINI, A.,et al, “Fibre properties and crashworthiness parameters of natural fibre-reinforced composite structure: a literature review”, Composite Structures, v. 148, pp. 59–73, 2016. doi: http://doi.org/10.1016/j.compstruct.2016.01.098.
    » https://doi.org/10.1016/j.compstruct.2016.01.098
  • [17] WU, Z., KHAYAT, K., SHI, C., “Changes in rheology and mechanical properties of ultra-high performance concrete with silica fume content”, Cement and Concrete Research, v. 123, pp. 105786, 2019. doi: http://doi.org/10.1016/j.cemconres.2019.105786.
    » https://doi.org/10.1016/j.cemconres.2019.105786
  • [18] KHORAMI, M., GANJIAN, E., “Comparing flexural behaviour of fibre-cement composites reinforced bagasse: wheat and eucalyptus”, Construction & Building Materials, v. 25, n. 9, pp. 3661–3667, 2011. doi: http://doi.org/10.1016/j.conbuildmat.2011.03.052.
    » https://doi.org/10.1016/j.conbuildmat.2011.03.052
  • [19] KADHAR, S.A., GOPAL, E., SIVAKUMAR, V., et al, “Optimizing flow, strength, and durability in high-strength self-compacting and self-curing concrete utilizing lightweight aggregates”, Matéria (Rio de Janeiro), v. 29, n. 1, pp. e20230336, 2024. doi: http://doi.org/10.1590/1517-7076-rmat-2023-0336.
    » https://doi.org/10.1590/1517-7076-rmat-2023-0336
  • [20] ABDELMOULEH, M., BOUFI, S., BELGACEM, M.N., et al, “Short natural-fibre reinforced polyethylene and natural rubber composites: effect of silane coupling agents and fibres loading”, Composites Science and Technology, v. 67, n. 7–8, pp. 1627–1639, 2007. doi: http://doi.org/10.1016/j.compscitech.2006.07.003.
    » https://doi.org/10.1016/j.compscitech.2006.07.003
  • [21] ZHOU, X., GUO, D., HUANG, S., et al, “A green, efficient and economical polypeptide—modified bamboo fiber and its application in glycopeptide antibiotics adsorption”, Cellulose (London, England), v. 30, n. 8, pp. 5201–5215, 2023. doi: http://doi.org/10.1007/s10570-023-05187-8.
    » https://doi.org/10.1007/s10570-023-05187-8
  • [22] PARTHASAARATHI, R., BALASUNDARAM, N., ARASU, N., “Analysing the impact and investigating Coconut Shell Fiber Reinforced Concrete (CSFRC) under varied loading conditions”, Journal of Advanced Research in Applied Sciences and Engineering Technology, v. 35, n. 1, pp. 106–120, 2024.
  • [23] PARTHASAARATHI, R., BALASUNDARAM, N., NAVEEN ARASU, A. “A stiffness analysis of treated and non-treated meshed coir layer fibre reinforced cement concrete”, In: AIP Conference Proceedings, v. 2861, n. 1, 2023. doi: http://doi.org/10.1063/5.0158672.
    » https://doi.org/10.1063/5.0158672
  • [24] SRINIVASAN, S.S., MUTHUSAMY, N., ANBARASU, N.A., “The structural performance of fiber-reinforced concrete beams with nanosilica”, Matéria (Rio de Janeiro), v. 29, n. 3, pp. e20240194, 2024. doi: http://doi.org/10.1590/1517-7076-rmat-2024-0194.
    » https://doi.org/10.1590/1517-7076-rmat-2024-0194
  • [25] KUMAR, S.N., NATARAJAN, M., NAVEEN ARASU, A. “A comprehensive microstructural analysis for enhancing concrete’s longevity and environmental sustainability”, Journal of Environmental Nanotechnology, v. 13, n. 2, pp. 368–376, 2024. doi: http://doi.org/10.13074/jent.2024.06.242584.
    » https://doi.org/10.13074/jent.2024.06.242584
  • [26] MOHD NURAZZI, N., KHALINA, A., CHANDRASEKAR, M., et al, “Effect of fiber orientation and fiber loading on the mechanical and thermal properties of sugar palm yarn fiber reinforced unsaturated polyester resin composites”, Polimery, v. 65, n. 2, pp. 115–124, 2020. doi: http://doi.org/10.14314/polimery.2020.2.5.
    » https://doi.org/10.14314/polimery.2020.2.5
  • [27] SHALWAN, A., ALSAEED, T., YOUSIF, B., “Machinability of polymeric composites and future reinforcements: a review”, Journal of Materials Science and Chemical Engineering, v. 10, n. 5, pp. 40–72, 2022. doi: http://doi.org/10.4236/msce.2022.105004.
    » https://doi.org/10.4236/msce.2022.105004
  • [28] MUNIANDY, M., MUSTAPA, S., ALI, N., et al “Effect of fibre treatment on tensile properties in bamboo fibre extraction: a review paper” In International Conference on Mechanical, System and Control Engineer, pp. 3–9, Singapore, 2021.

Correspondence

Corresponding Author: Nandagopalan Subban. e-mail: civilnandagopalan.s@gmail.com, pmnatarajanin@gmail.com, balasundaram49@gmail.com

Publication Dates

  • Publication in this collection
    11 Nov 2024
  • Date of issue
    2024

History

  • Received
    12 Aug 2024
  • Accepted
    24 Sept 2024
location_on
Laboratório de Hidrogênio, Coppe - Universidade Federal do Rio de Janeiro, em cooperação com a Associação Brasileira do Hidrogênio, ABH2 Av. Moniz Aragão, 207, 21941-594, Rio de Janeiro, RJ, Brasil, Tel: +55 (21) 3938-8791 - Rio de Janeiro - RJ - Brazil
E-mail: revmateria@gmail.com
rss_feed Acompanhe os números deste periódico no seu leitor de RSS
Ir para o topo