Open-access Durability characteristics on Self-Compacting Concrete using casting slag as fine aggregate

ABSTRACT

Self-Compacting Concrete (SCC) is a very flexible concrete that flows through intricate, heavily reinforced structural components and compacts under its own weight. Natural sand is in extremely high demand in developing countries because of the rapid expansion of the infrastructure. Many researchers are substituting some of the fine aggregate with materials based on slag. Environmental contamination is increased by the production of casting slag, a by-product of the casting industries that can be used to make concrete. Casting slag is a coagulation process result that is a solid in the iron industry. After being identified as garbage, it is usually disposed of in the utility disposal site. As a result, an effort has been undertaken to assess how casting slag affects the amount of Fine Aggregate (FA) replacement in the percentage of be 0%, 10%, 20%, and 30% and abovementioned tests were conducted. The results of the tests demonstrated that casting slag may be utilized efficiently as a substitute in part for fine aggregate in self-compacting concrete, resulting in sustainable construction.

Keywords:
Self-Compacting Concrete; Workability; Durability; Casting Slag; Fine Aggregate

1. INTRODUCTION

Statistics studies show that a significant number of environmentally harmful compounds are discharged into the environment annually along with a rise in the production of solid trash. One ton of solid trash is produced for every ton of crude steel manufactured. 29 million tonnes of slag are disposed annually by large-scale steel- producing industries. For the 63 nations that report to the World Steel Association, the total amount of crude steel produced worldwide was 158.8 million tonnes (Mt). While there is a marginal 0.1% decrease compared to June 2022, it is important to note that this small decline cannot be viewed as a significant factor in mitigating the environmental impact caused by the disposal of slag [1]. In India even though cement industries are utilizing slag wastes, compressive amount of slag is produced annually with increase in metal production industries with increase in usage of metals in day-to-day activities.

In areas where achieving proper vibration is challenging, concreting can lead to uneven compaction, adversely affecting both permeability and concrete durability. This drawback spurred the development of Self- Compacting Concrete (SCC). First developed in 1988, SCC aims to produce concrete constructions with increased durability [2, 3]. It was developed in Japan and presented practically in Sweden in mid-1990’s. Contributing a good strength and durability by providing a smoother finish to the concrete structures, it also reduces quite significant amount of noise pollution produced in compacting concrete. Must be easy flowing and homogenous in nature neglecting segregation. Four primary metrics may be used to assess the stability of Self- Compacting Concrete (SCC): flowability, viscosity, passing ability, and segregation resistance. Limestone, fly ash, and silica fumes are among the materials used to increase cohesion and decrease segregation. Hyper plasticizers or viscosity-modifying additives lessen the segregation and sensitivity of concrete. Diffusion of flocculated particles should occur concurrently with water binding and wetting. Included is a third-generation superplasticizer that is made with a poly-carboxylic ether basis. Slags and other by-products were introduced with variations in SCC, which prompted researchers worldwide to conduct several studies in this area. Despite the various benefits, typical SCC composites crack propagation, mechanical strength, formability, and crack resistance are restricted. Metal slag SCC combination provides effective protection against chloride ion penetration. Comparatively to SCC combinations without iron slag, the cumulative charge that was transferred through iron slag mixtures was lower [4].

Research into using casting slag, or slag inclusions, it has been made feasible by this concept to substantially replace fine particles in self-compacting concrete. Non-metallic elements can cause pockets or ribbon-like entrainments in the casting, which is known as slag inclusion [5]. Slag is a crucial component of the melting process in the furnace and is required for high-quality castings because chemical reactions in silica and calcium- based slags alter the metal’s viscosity. Casting slag is primarily composed of slag inclusions. Low-viscosity slags ascend to the casting surface where the defect forms considerably more quickly than high-viscosity slags do in the solidified casting structure. The irregular shape of slag inclusions, which can include melt slags, carbide slags, and treatment slags, reveals their origin and composition [6]. Incorporating Slag variants in SCC have led many researchers come to a significant conclusion that slag in SCC has contributed to various sustainable results.

The incorporation of casting slag in self-compacting concrete (SCC) not only addresses the growing demand for sustainable construction materials but also contributes significantly to reducing environmental challenges posed by industrial by-products. By utilizing casting slag as a partial replacement for fine aggregates, this approach minimizes the reliance on natural sand, conserves diminishing natural resources, and diverts substantial quantities of slag from landfills. Additionally, the recycling of casting slag reduces the carbon footprint associated with the production and disposal of traditional concrete materials, aligning with global efforts to promote a circular economy. This innovative use of casting slag in SCC enhances workability and durability while simultaneously advancing the goals of eco-friendly construction.

2. EXPERIMENTAL INVESTIGATION

2.1. Materials

2.1.1. Cement

For the investigation, Ordinary Portland Cement (OPC) grade 43 that complies with [7] was utilized. Table 1 presents the basic characteristics of the cement and includes a full breakdown of its features.

Table 1
Physical characteristic of cement and flyash.
2.1.2. Fly ash

Used was Class-F fly ash from a local coal power station. It possessed particles smaller than 45 µm and exhibited a grey coloration. It had a 2.24 specific gravity [8].

2.1.3. Casting slag

Slag inclusions were bought from nearby foundry [9, 10]. Specific gravity of casting slag is 2.42 respectively.

2.1.4. Superplasticizer

Aura-mix 400 is an excellent blend of cutting-edge superplasticizers. It is based on a long side chain polymer of polycarboxylic ether. This product is a clear, pale-yellow liquid with a minimum pH of 6.0 and no chlorides.

2.1.5. Coarse and fine aggregate

The 12 mm-sized gravel, which was easily accessible in the area and had a specific gravity of 2.69 and a fineness modulus of 6.87, was used to create the coarse aggregate. For the fine aggregate, crushed stone sand with particles smaller than 4.75 mm and a fineness modulus of 2.64 was employed.

2.1.6. Proportion

Several test mixtures were created in order to confirm compliance with SCC regulations as stated in GUPTA and SIDDIQUE [11]. Table 2 lists the amounts of fly ash, cement, fine aggregate, and coarse aggregate.

Table 2
Proportioning of SCC incorporating casting slag.
2.1.7. Test procedures

After conducting a significant number of trials in accordance with the guidelines [6], the final design mix was determined. Before casting, various tests were performed, including the slump flow test, L-box test, and V-funnel test, to evaluate the flowability, viscosity, passing ability, and segregation resistance of the SCC specimens. The compressive strength of the concrete was assessed using 150 mm cubes after 7, 28, and 90 days of curing, in accordance with the specified standards [12]. Additionally, split tensile strength, flexural strength, and water absorption were evaluated at 7, 28, and 90 days, following the relevant guidelines [8, 13].

3. RESULTS AND DISCUSSIONS

3.1. Fresh properties

The new characteristics of SCC using the Slump flow, V funnel, and L box tests. The viscosity and passing ability were determined using the V-funnel and L-box tests, while the filling capacity was evaluated using the slump flow test. Table 3 outlines the range and class of SCC based on the slump flow value [12, 14].

Table 3
Fresh properties of SCC with different casting slag percentages.

The viscosity of fresh concrete was indirectly determined through the V-funnel test, which measured the rate of flow. Concrete was poured into the funnel until it reached the top, and the amount of time needed to drain the funnel was noted. Concrete viscosity was classified according to the EFNARC recommendations based on the flow time in the V-funnel [15].

3.2. Hardened concrete properties

3.2.1. Compressive strength

Cubic specimens of 100 × 100 × 100 mm underwent compression strength testing after 7, 28, 90 days of curing. Using compression testing apparatus capable of testing 2000 tons, triplicates of the compressive test were performed for each curing period in accordance with [16]. In reality, the strength increase is a positive attribute of the interfacial transition zone over the aggregate and not just a source of the rigidity of changing aggregates. Compressive strengths of the SCC control mixture without casting slag were 31.56 MPa and 31.96 MPa at days 28, 90, and 90, respectively. After 28 days, the SCC mixes with 10, 20, and 30% casting slag added as fine aggregates showed increases in compressive strength of 0.89%, 3%, and 1.8%, respectively, above Control SCC (no casting slag). SCC mixes comprising 10, 20, and 30% iron slag as fine aggregates obtained 0.81%, 2.75%, and 1.88% greater compressive strength after 90 days than 90 days SCC mixture (without casting slag).

Compressive strength increased across the board as casting slag content increased, indicating that the SCC became denser as a result of the addition of casting slag. Comparing SCC with casting slag to control concrete at 90 days, there was a 2.75% improvement in compressive strength. According to concrete that replaces 20% of its natural aggregates with casting slag aggregates has greater compressive strength than control concrete that uses only natural aggregates. Positive outcomes are obtained when casting slag is substituted by more than 20% (Figure 1).

Figure 1
Compressive strength for different mix proportion.
3.2.2. Split tensile strength

Casting slag was gradually added to SCC, bringing its compressive strength up to 50%; further addition weakens the material. The tendency has also been observed in the other two strength metrics, namely tensile and flexural strength. When 20% of the fine aggregate was replaced with casting slag, all the strength criteria demonstrated a significant improvement. The split tensile strength at 14- and 28-days curing period. Comparing the tensile strength of the mix proportions at 10%, 20% and 30% replacements to the control mix at 14 days, the gains are 1.23%, 1.85%, and 0.62%, respectively. In line with the compressive strength, the split tensile strength for mix at 20% likewise had a little increase; however, there is a sharp increase in strength from 10% to 20% and 20% to 30%, rising by 0.55% and 1.09% over the course of 28 days, respectively. The ideal ratio for replacing some of the fine aggregate with casting slag is ultimately determined to be 20% (Figure 2).

Figure 2
Split tensile strength for different mix proportion.
3.2.3. Water absorption

Concrete’s water permeability has a big impact on how long it lasts. Concrete’s water absorption capacity may be used as a basic indicator of how resilient it is to hostile situations. Up to ninety days of observation were conducted on the water absorption outcomes of casting slag in SCC blends. The water absorption for the SCC mixture without replacing the casting slag with fine aggregates was 4.81% after 28 days, and it dropped to 4.12% after 90 days. According to the results, the percentage of water absorption falls for all concrete compositions as the amount of casting slag increases.

The same is true for curing age because water absorption lowers as time goes on. Following a 7-day curing period, SCC mixtures with fine aggregates containing 10, 20, and 30% casting slag absorbed 1, 3, and 9% less water than those without casting slag. 28-day-old SCC mixtures with fine aggregates containing 10, 20, and 30% casting slag obtained 1.66, 12.05, and 17.67% less absorption than 28-day-old SCC mixtures without casting slag. SCC combinations with 10, 20, and 30% casting slag as fine aggregates at 90 days absorbed 1.21%, 5.58%, and 8% less water than 90-day SCC mixtures without casting slag (Figure 3).

Figure 3
Water Absorption for different mix proportion.

4. CONCLUSION

This purpose of this study was to evaluate SCC’s fine aggregate composition and durability of SCC. The primary conclusions of this investigation are as follows.

  • It was noted that the increase in casting slag improved SCC’s fresh characteristics. The use of casting slag enhanced Viscosity, passing, and filling ability.

  • Compared to control concrete, SCC mixtures with up to 20% slag had an increase in strength. Still, the strength improvement was about the same with a 20% substitution of slag.

  • After 7th day, the compressive strength of the control concrete reached its maximum. The highest compressive strength was seen at 20% replacement throughout the remaining curing ages, and strength declined with increased substitution.

  • In SCC, water absorption was significantly reduced by replacing up to 20% casting slag. However, SCC mixes with 20% replacement slag exhibited the lowest absorption values. The rate of absorption for SCC with 20% casting slag reduced by 1, 3, and 9% at ages 7, 28, and 90 days respectively. SCC with more than 20% slag did not absorb water more than control concrete.

  • These improvements minimize the need for mechanical compaction, particularly in areas with dense reinforcement, reducing labour and equipment costs. Additionally, the self-levelling nature of SCC with higher slag content ensures uniform placement and finishes, even in complex geometries.

5. BIBLIOGRAPHY

  • [1] ADEBANJO, A.U., KAREEM, M.A., OLATOYAN, O.J., et al, “Assessing the durability properties of sandcrete blocks incorporating iron filings as fine aggregate”, Hybrid Advances, v. 6, pp. 100228, 2024. doi: http://doi.org/10.1016/j.hybadv.2024.100228.
    » https://doi.org/10.1016/j.hybadv.2024.100228
  • [2] BIRGONDA, S., SENTHILKUMAR, R., RAMESH, S.T., “Induction furnace slag as fine and coarse aggregate in quaternary blended self-compacting concrete: a comprehensive study on durability and performance”, Materials Today Sustainability, v. 27, pp. 100873, 2024. doi: http://doi.org/10.1016/j.mtsust.2024.100873.
    » https://doi.org/10.1016/j.mtsust.2024.100873.
  • [3] [3] BAYAT, H., BANAR, R., NIKRAVAN, M., et al, “Durability, mechanical, workability, and environmental assessment of self-consolidating concrete containing blast furnace slag and natural zeolite”, Journal of Building Engineering, v. 86, pp. 108737, 2024. doi: http://doi.org/10.1016/j.jobe.2024.108737.
    » https://doi.org/10.1016/j.jobe.2024.108737
  • [4] [4] KUMAR, S., SAHU, A., SRIVASTAVA, A.K.L., “Effect of copper slag on recycled aggregate based self-compacting concrete”, Materials Today: Proceedings, v. 93, n. Part 3, pp. 480–488, 2023. doi: http://doi.org/10.1016/j.matpr.2023.08.151.
    » https://doi.org/10.1016/j.matpr.2023.08.151
  • [5] DHARMARAJ, R., DHIVAKARAN, P.N., KARUPPASAMY NARAYANAN, R., “Strength characteristics properties of papaya leaf extract as green inhibitor in concrete”, Materials Today: Proceedings, v. 68, n. Part 6, pp. 2368–2374, 2022. doi: http://doi.org/10.1016/j.matpr.2022.09.104.
    » https://doi.org/10.1016/j.matpr.2022.09.104
  • [6] SOSA, I., THOMAS, C., POLANCO, J.A., et al, “Durability of high-performance self-compacted concrete using electric arc furnace slag aggregate and cupola slag powder”, Cement and Concrete Composites, v. 127, pp. 104399, 2022. doi: http://doi.org/10.1016/j.cemconcomp.2021.104399.
    » https://doi.org/10.1016/j.cemconcomp.2021.104399
  • [7] BUREAU OF INDIAN STANDARDS, BIS 8112-2013 Ordinary Portland cement, 43 Grade-Specification, New Delhi, BIS, 2013.
  • [8] SHARMA, R., KHAN, R.A., “Sulfate resistance of self-compacting concrete incorporating copper slag as fine aggregates with mineral admixtures”, Construction & Building Materials, v. 287, pp. 122985, 2021. doi: http://doi.org/10.1016/j.conbuildmat.2021.122985.
    » https://doi.org/10.1016/j.conbuildmat.2021.122985
  • [9] SINGH, G., SIDDIQUE, R., “Effect of iron slag as partial replacement of fine aggregates on the durability characteristics of self-compacting concrete”, Construction & Building Materials, v. 128, pp. 88, 2016. doi: http://doi.org/10.1016/j.conbuildmat.2016.10.074.
    » https://doi.org/10.1016/j.conbuildmat.2016.10.074
  • [10] DE SCHEPPER, M., VERLÉ, P., VAN DRIESSCHE, I., et al, “Use of secondary slags in completely recyclable concrete”, Journal of Materials in Civil Engineering, v. 27, n. 5, pp. 04014177, 2015. doi: http://doi.org/10.1061/(ASCE)MT.1943-5533.0001133.
    » https://doi.org/10.1061/(ASCE)MT.1943-5533.0001133
  • [11] GUPTA, N., SIDDIQUE, R., “Durability characteristics of self-compacting concrete made with copper slag”, Construction & Building Materials, v. 247, pp. 118580, 2020. doi: http://doi.org/10.1016/j.conbuildmat.2020.118580.
    » https://doi.org/10.1016/j.conbuildmat.2020.118580
  • [12] MOHAPATRU, J.K., CHANDRASEKHAR, B.P.R., Roads, I.I. Report, New Delhi, Oxford University Press, p. 109-137, 2007.
  • [13] CHANDRU, P., KARTHIKEYAN, J., SAHU, A.K., et al, “Some durability characteristics of ternary blended SCC containing crushed stone and induction furnace slag as coarse aggregate”, Construction & Building Materials, v. 270, pp. 121483, 2021. doi: http://doi.org/10.1016/j.conbuildmat.2020.121483.
    » https://doi.org/10.1016/j.conbuildmat.2020.121483
  • [14] SHEEN, Y.N., LE, D.H., SUN, T.H., “Greener self-compacting concrete using stainless steel reducing slag”, Construction & Building Materials, v. 82, pp. 341–350, 2015. doi: http://doi.org/10.1016/j.conbuildmat.2015.02.081.
    » https://doi.org/10.1016/j.conbuildmat.2015.02.081
  • [15] European Federation of Specialist Construction Chemicals and Concrete Systems, Guidelines for self-compacting concrete, London, EFNARC, v. 32, p. 34, 2005.
  • [16] BUREAU OF INDIAN STANDARDS, BIS 516-1959 Method of Tests for Strength of Concrete, New Delhi, BIS, 1959.

Publication Dates

  • Publication in this collection
    21 Feb 2025
  • Date of issue
    2025

History

  • Received
    23 Nov 2024
  • Accepted
    06 Dec 2024
location_on
Laboratório de Hidrogênio, Coppe - Universidade Federal do Rio de Janeiro, em cooperação com a Associação Brasileira do Hidrogênio, ABH2 Av. Moniz Aragão, 207, 21941-594, Rio de Janeiro, RJ, Brasil, Tel: +55 (21) 3938-8791 - Rio de Janeiro - RJ - Brazil
E-mail: revmateria@gmail.com
rss_feed Acompanhe os números deste periódico no seu leitor de RSS
Ir para o topo