ABSTRACT
This study explores the influence of nanosilica on the mechanical and durability properties of high-performance concrete (HPC) incorporating pineapple leaf fiber (PALF) as secondary reinforcement, with an optimum PALF content of 2.5%. Simultaneously, nano-silica was used to partially replace Portland cement at levels of 0.5% to 2.5 wt.%. Concrete mixtures were evaluated for workability, sorptivity, rapid chloride ion penetration, water absorption, compressive strength, flexural strength, splitting tensile strength, and abrasion resistance. The addition of nano-silica enhanced the overall mechanical and durability performance of HPC, with optimal benefits observed at a 2 wt.% replacement level. However, increasing nano-silica content led to higher water demand due to its high specific surface area, although consistent workability was maintained using superplasticizers. Nano-silica functioned both as a pozzolanic activator and micro-filler, refining the microstructure and enhancing interfacial bonding. Microstructural analyses using scanning electron microscopy (SEM), X-ray diffraction (XRD), and Fourier-transform infrared spectroscopy (FTIR) confirmed the improved matrix density and reduced porosity. The combined use of PALF and nano-silica demonstrates strong potential for sustainable and durable structural applications in HPC.
Keywords:
Pineapple leaf fiber; Nano-silica; High-Performance Concrete; Durability; Concrete Properties
1. INTRODUCTION
The growing demand for durable and sustainable infrastructure has accelerated the use of advanced construction materials, among which high-performance concrete (HPC) plays a vital role. HPC has been widely utilised in the past three decades due to its superior strength, durability, and adaptability to modern construction requirements. Its compressive strength typically ranges from 18 to 200 MPa; however, performance is not defined by strength alone. Workability and durability are equally critical to ensuring the long-term reliability of HPC in diverse applications [1]. One of the most effective methods of enhancing HPC properties is through the incorporation of nanosilica. Available in both dry powder and colloidal solution forms, nanosilica can significantly improve concrete performance even at low replacement levels, generally within 0–6%. Its addition accelerates the hydration process, increases the formation of calcium–silicate–hydrates (C–S–H), and reduces calcium hydroxide crystals, resulting in a denser and more compact microstructure [2, 3]. At replacement levels up to 3%, nanosilica exhibits strong pozzolanic reactivity [3]. Consequently, nanosilica-modified concrete demonstrates substantial improvements in compressive, flexural, and split tensile strengths [4], along with enhanced abrasion resistance compared to conventional concrete [5]. Furthermore, as the endurance of concrete increases, its microstructure becomes denser. Studies on nanosilica-modified concrete have reported significant improvements in flexural and tensile strengths, along with reductions in water absorption, permeability, and capillary action [6]. Nanosilica also decreases the time required to achieve initial and final setting, shortens the dormant phase of hydration, and reduces chloride ion penetration in mixes containing fly ash and slag [7]. In addition, its incorporation accelerates hydration reactions, thereby enhancing early-age compressive strength. For example, the inclusion of nanosilica with ceramic waste powder was found to improve strength development at early stages [8]. However, while nanosilica contributes positively to early-age performance, it may inhibit strength development at later ages. In high-volume fly ash concrete, nanosilica not only refines hydration during the dormant phase but also improves resistance to chloride penetration and reduces setting times, further contributing to improved mechanical performance [9].
When nanosilica in recycled aggregate concrete, the strength increased compared to unrecycled aggregate concrete [10]. The use of nanoparticle reduced the strength and setting time of oil well cement [11]. Nanosilica can be used to reduce the unfavourable impact of sludge inclusion on mortar setting time [12]. Evidence suggests that adding nano-silica to cement composites increased strength by almost 15–20% [13]. Furthermore, nano silica particles improve the abrasion, impact, and water absorption resistance of sludge/clay mixes used to make tiles [14]. Nano-silica improves the durability of concrete because of its greater surface area and very less particle size. Nanosilica fills the small crevices in the cement to form a thick framework, while hydration nanosilica and calcium hydroxide produces additional gel formation [15]. Silica nanoparticle, with its massive surface area, is the focal point of phase transition, which improves hydration [16]. Increased nanosilica content promotes buildup, preventing uniform nanosilica particle distribution within the mortar. As a result, quantity of nano particle increases, increase in compressive strength decreases due to more effective adsorption of Ca+2 ions and reduction in calcium ion concentration. Nanoparticles accelerate the breakdown of C3S and increase hydration [17]. Aggregate and cement adhere to each other more strongly. Nano silica powder is more convenient and efficient to introduce than nano silica colloidal [18]. Nanotechnology appears to have more promise in two areas: construction and building materials. Therefore, understanding nanotoxicology is crucial. As nano silica concentrations rise, the gain in compressive strength begins to drop [19].
In the pursuit of sustainable and high-performance construction materials, pineapple leaf fiber (PALF)—a readily available agricultural byproduct—has garnered considerable interest as a natural reinforcement for cement-based composites. Its abundant cellulose content, impressive tensile strength, and crack-bridging capacity make it a compelling choice to enhance the brittleness and durability of conventional concrete [20]. Recent experimental studies have further substantiated PALF’s effectiveness: for instance, treated fibers have been shown to significantly improve compressive and flexural strength at optimized dosages, while stringent factorial designs have revealed that alkali treatment can enhance fiber–matrix bonding, notably increasing tensile and flexural performance in cementitious matrices [21]. Moreover, comprehensive reviews underscore PALF’s ability to arrest crack propagation, augment toughness, and boost split tensile strength in engineered cementitious composites, although its influence on workability necessitates mix design adjustments [22].
This study focuses on enhancing the mechanical and durability properties of High-Performance Concrete (HPC) through the incorporation of nanosilica (NS), silica fume (SF), and pineapple leaf fiber (PALF). The goal is to develop concrete with superior compressive strength, tensile strength, and improved resistance to environmental degradation, thereby offering more durable and reliable construction materials for a broad range of infrastructure applications. A key aspect of the research is the evaluation of PALF, a natural and sustainable material, as a secondary reinforcement. This contributes to more sustainable construction practices by lowering the carbon footprint of concrete production and promoting the use of eco-friendly alternatives in the industry. The study also investigates the long-term performance of the modified HPC by assessing its durability under various environmental stressors, including chloride-ion penetration, water absorption, abrasion resistance, sorptivity, and chemical attacks. This aims to extend the service life of concrete structures, particularly those exposed to aggressive environments such as marine infrastructure, highways, and bridges.
2. MATERIALS AND METHODS
By I.S. 12269:1987, the appropriate Portland Cement of Grade 53 were used. The cement specific gravity is 3.16 and Chemical state Properties are included in Table 1. River sand was selected for fine aggregate because of its 2.66 specific gravity and 2.91 fineness modulus. It conforms with zone II of I.S.: 383-1970 and has a bulk density of 1780 kg/m3. For the investigation, pineapple leaves were manually chopped to 2 cm in length and tested before being employed in concrete, where the fibers exhibited a density of 1.31 g/cm3, a Young’s modulus of 14.30 GPa, and an elongation at break of 1.40%. The research used crushed granite coarse aggregate with a bulk density of 1650 kg/m3 and specific gravity of 2.73, providing a maximum size of 12.5 mm aggregate. Conplast SP430 superplasticizer, was employed. It complies with IS 9103: 1999 standards, had a specific gravity 1.09, a relative density value 1.08 ± 0.02, and a pH of superplasticizer higher than 6. Figures 1(a) and 1(b) shows the findings for the size and shape of nano-silica determined using the X-ray Diffraction (XRD) and Scanning Electron Microscopy (SEM) respectively. Treated Fibers with alkali and silane. These treatments were carried out to remove surface impurities, enhance fiber–matrix bonding, and improve durability in the alkaline cementitious environment. For bonding with cement, PALF were incorporated at varying percentages by mass of cement: 0%, 0.5%, 1%, 1.5%, 2%, 2.5%, and 3%. The results demonstrate that the addition of PALF significantly enhances the compressive strength of the mortar, with the maximum improvement observed at 2.5% fiber content by weight. Based on this finding, 2.5% was maintained as a constant in subsequent processes.
2.1. Mix design
The mix proportioning technique given in ACI method was used to establish the mix design proportion for M60 grade concrete. Six concrete mixtures were made for 100 mm to 150 mm workability using Pineapple leaf fiber at 2.5 percent, whereas the amount of nano-silica was 0.5, 1, 1.5, 2 and 2.5 percentage, respectively. However, the w/c ratio in all concrete compositions was maintained at 0.31. In addition, the superplasticizer (1%) in each mix were maintained to keep the slump within the desired range. Table 1 displays the mix ratio selected for the investigation.
3. RESULTS AND DISCUSSIONS
Silica nanoparticle in concrete compressive strength with a consistent 2.5% substitution of Pineapple leaf fiber is shown in Table 2. Every nano silica blend has more strength than the control mixtures. Including nano-silica, up to 2% enhanced the strength of concrete before causing them to weaken. Comparison reference mix MPN0, the compressive strength of cubes increased by 25.8%, 52.81%, 81%, 100.5% and 95% for the NS0.5, NS1, NS1.5, NS2 and NS2.5 mixes respectively. The high tendency of nanoparticles to aggregate when mixed with water affects cement-based products properties. Therefore, the ideal amount of nano silica is limited by the development of accumulation caused by the ineffective dispersion of nano particles. Due to ITZ densification and filling effects, cementitious nano-silica systems have improved compressive strength.
Figure 2 shows how the adding nano-silica to material changed the splitting tensile strength across all grade levels. At 7 days, NS0.5, NS1, NS1.5, NS2 and NS2.5 shows an increase split tensile value of 3.76%, 9%, 14.5%, 18.6% and 15.7% respectively, compared to the ordinary mixture NS0. For the NS0.5, NS1, NS1.5, NS2 and NS2.5 mixes, the tensile strength attained after 7 days was 5.1%, 10.41%, 16.3%, 21% and 18.1% higher than the control NS0 shown in Figure 3. The HPC, which has silica added, has splitting tensile strengths that are substantially higher than those of the ordinary mix because the cement paste, and aggregate are better bound than in the control mix.
Figure 4 shows how the adding of nano-silica affects flexural strength across all ages. NS0.5, NS1, NS1.5, NS2 and NS2.5 had increased flexural strength of the beam by 16%, 24.4%, 32.6%, 41% and 32.9% respectively, after 7 days in contrast to the PN0 mix. The control mix NS0 7-day flexural strength was found to be 6.26 MPa, and for the NS0.5, NS1, NS1.5, NS2 and NS2.5 mix, the flexural strength increase over the control mix PN0 was found to be 11.8%, 20.1%, 29.4%, 37.7% and 33.1% respectively.
Table 2 results clearly show that mixes with higher percentages of nanosilica (NS) particularly the NS2 mixes offer significantly greater resistance to chloride ion (Cl−) penetration compared to the control mix. For instance, the NS2 mix registered just 1112 Coulombs at 28 days, indicating a marked decrease in permeability. Similarly, the mix with NS2.5 achieved an impressive value of 1365 Coulombs at the same age. These reductions highlight the role of higher NS content in producing a denser concrete matrix, which effectively limits chloride ingress and enhances long-term durability.
The molecular bands in the specimens with and without Nano Particle at 28 days of curing were evaluated using FTIR analysis, as shown in Figure 5. There are four sections to the Fourier transom infrared spectroscopy spectrum. The ranges in which these segments were seen are 3530–1810, 1475–1250, 1155–950, and 875–470 cm–1. Except for Ca(OH)2, molecular sets in the concrete specimen with and without nanosilica are almost infinite in terms of wavenumber. Percentage of nano particle increases, less water is available due to absorption, which permits the formation of CSH gel. The production of calcium hydroxide as a result of the development of gel increased the rate of addition to ideal rate (NS2 mixture). With the same degree of polymerization, the calcium hydroxide that was produced changed further into the CSH gel.
As the nanosilica value increases from 0 (no additive) to 2.5, the intensity of the O–Si–O peak (~1100 cm−1) increases, indicating increased silica content in the samples. The intensity of the C–S–H band (~960 cm−1) also increases with the addition of nano-silica, suggesting enhanced formation of C–S–H gel due to the pozzolanic reaction between nano-silica and calcium hydroxide. Correspondingly, the Ca(OH)2 peak (~3640 cm−1) decreases slightly with increasing nano-silica content, implying that calcium hydroxide is consumed during the pozzolanic reaction to form additional C–S–H.
Figure 6 shows the spectra of specimen made up of different amounts of nano silica, and Pineapple leaf fiber as well as the intensity and 2 theta degrees of the reference combination. A decrease in Gypsum, C3S, C2S and C3A were all found in the reference combinations in greatest concentrations. The hydration of binder results in the generation of hydration products such as C-S-H lime and Ca(OH)2 which is responsible for this drop in peak values. Due to the amorphous nature of silica, the peaks may be activated to C-S-H gel, which are measured in small amounts. Nanosilica concrete, as shown in Figure 6(b-e), showed XRD data with high peaks in comparison to control combination. This demonstrates that the presence of pineapple leaf fiber did not prevent the binder chemicals from hydrating. The study carried out on reaction of silica in cementitious composites has found that nano silica hydrates effectively. The XRD results reveal that the incorporation of nano-silica significantly influences the hydration process of cement. The control mix (NS0) shows high Ca(OH)2 intensity, while with increasing NS content, portlandite peaks gradually reduce and C-S-H and CaCO3 phases become more pronounced, indicating enhanced pozzolanic activity. At moderate dosages (1–1.5%), the reduction of Ca(OH)2 and growth of C-S-H are most evident, suggesting effective utilization of lime and improved microstructural refinement. At higher additions (2–2.5%), further consumption of Ca(OH)2 and increased C-S-H are observed, though possible agglomeration of nanoparticles may limit uniformity. Overall, nano-silica promotes secondary hydration and densification, with optimum performance around 1.5–2%.
XRD analysis of specimen (a) NS0 mixture (b) NS0.5 mixture (c) NS1 mixture (d) NS 1.5 mixture (e) NS2 mixture (f) NS 2.5 mixture.
The microstructural characterization, which is still being thoroughly investigated, determines the concrete’s strength and rheological characteristics. Figure 7 displays the micrographs from the SEM analysis of typical nano silica and fiber specimens. The calcium-hydrated phases are found in portlandite, calcite, and C-S-H. For specimen NS0, Figure 7(a) depicts the lack of thick C-S-H gel but there is abundance of Ca (OH)2, ettringite, and CaCO3. Given that holes were extensively spaced and that hairline fractures could be seen propagating through the concrete matrix, the link between the particles was highly undesired. Although there is a minor improvement in the dense C-S-H gel formation, the visualization for the fiber and nano silica-made combination (NS2) is identical. A significant decrease in pores and voids, compared to NS0, is shown in Figure 7(a), which illustrates the existence of ettringite and calcium iron silicates (Hedenbergite).
SEM photographs of the specimen (a) NS0 mixture (b) NS0.5 mixture (c) NS1 mixture (d) NS1.5 mixture (e) NS2 mixture (f) NS 2.5 mixture.
Figure 8 illustrates the nano-silica impact on the water absorption of HPC mixes at 28 days and 90 days. When replacing 2% of cement by silica, the water absorption reduced from 2.98% to 1.94% and then slightly rise to 2.16% for 2.5% replacement of nanosilica at 28 days. Water absorption was 1.94% at 28 days and 1.53% at 90 days when 2% nano-silica was partly replaced. At both 28 and 90 days, none of the mixtures had significantly more water absorption than the control mixture. The properties of water absorption after 90 days continued along the same path due to nano silica, greater pozzolanic action made the concrete denser.
Nanosilica impact on the sorptivity of HPC mixtures is seen in Figure 9. As a measurement of amount of moisture transported into unsaturated specimens, sorptivity is now regarded as a key indicator of concrete durability. The sorptivity test uses capillary suction inside the concrete pore spaces rather than pressure heads to drive water into the Concrete. Therefore, the sorptivity coefficient is a crucial variable to consider while estimating the lifespan of a concrete building. The sorptivity value decreases by 43.21% in 28 days and 57% in 90 days, respectively, as the silica concentration rises from 0% to 2%. Nanosilica, made up of very small particles, reduces the capillary holes by filling the pores in cement paste. Therefore, adding nano-silica to concrete may increase its strength and decrease its capillary sorption.
The HPC with nano-silica incorporation was tested for abrasion resistance by measuring the amount of wear at 28 and 90 days. For all mixtures, the variance in wear depth after 1 h of testing The depth of wear reduced as concrete age increased for all mixes. Indicating that the increased levels had improved the abrasion resistance wear for 0.5% to 2.5% nano-silica as the result of the abrasion test were 1.54 mm, 1.38 mm, 1.2 mm, 0.73 and 0.91 mm respectively. Conventional mix’s wear depth was 1.98 mm at 28 days. Concrete mixtures incorporating nano-silica showed a significantly enhanced resistance to abrasion. The acceleration of nano silica pozzolanic activity and the increased concrete strength, notably in the ITZ, are the causes of the impact mentioned above. Up to a 2% weight replacement, the wear depth is reduced thereafter, marginally in increasing trend. When 2% nano-silica was substituted for cement in HPC mixes, abrasion resistance increased by around 63.6 and 71.85 percent above the control mix at 28 and 90 days, respectively.
4. CONCLUSIONS
-
Increasing the nano-silica content to 2.5% accelerated hydration, which resulted in higher consistency and reduced setting time. Incorporation of nano-silica in cement mortars containing 2.5% pineapple leaf fiber improved compressive strength at all curing ages.
-
Strength development increased up to 2% nano-silica, after which a slight decline was noted, though the values remained higher than those of the reference mix.
-
Slump test results indicated reduced workability with increasing nano-silica content due to its high surface area and greater water demand; however, suitable superplasticizer adjustments maintained consistency comparable to the control mix.
-
The presence of nano-silica enhanced early-stage pozzolanic activity, contributing significantly to long-term strength development and achieving compressive strengths 0.37–0.44 times greater than conventional mixes at 28 days.
-
The optimum dosage of 2% nano-silica produced the maximum gains in compressive, split tensile, and flexural strengths, attributed to the formation of additional C–S–H gel and a refined, denser microstructure.
-
Durability performance improved considerably, as reflected in very low RCPT values at 28 and 90 days, indicating reduced chloride ion penetration due to enhanced particle packing from both nano-silica and pineapple leaf fiber.
-
The pore-refining effect of nano-silica decreased water absorption and sorptivity, with the most notable reductions recorded at 2% dosage. Abrasion resistance increased with nano-silica incorporation up to 2%, where the lowest wear depth was achieved, followed by a slight decline at higher dosages.
5. BIBLIOGRAPHY
-
[1] BASSUONI, M.T., TIAN, Y., SAID, A.M., et al, “Properties of concrete using nano-silica”, Construction & Building Materials, v. 36, pp. 838–844, 2012. doi: http://doi.org/10.1016/j.conbuildmat.2012.06.044.
» https://doi.org/10.1016/j.conbuildmat.2012.06.044 -
[2] SINGH, L.P., KARADE, S.R., BHATTACHARYYA, S.K., et al, “Beneficial role of nanosilica in cement based materials: a review”, Construction & Building Materials, v. 47, pp. 1069–1077, 2013. doi: http://doi.org/10.1016/j.conbuildmat.2013.05.052.
» https://doi.org/10.1016/j.conbuildmat.2013.05.052 -
[3] NAJIGIVI, A., RASHID, S.A., AZIZ, F.N., et al, “The effects of lime solution on the properties of SiO2 nanoparticles binary blended concrete”, Composites. Part B, Engineering, v. 42, n. 3, pp. 562–569, 2011. doi: http://doi.org/10.1016/j.compositesb.2010.10.002.
» https://doi.org/10.1016/j.compositesb.2010.10.002 -
[4] JI, T., “Investigations on the development of the permeability properties of binary blended concrete with nano-SiO2 particles”, Cement and Concrete Research, v. 35, pp. 1943–1947, 2005. doi: http://doi.org/10.1016/j.cemconres.2005.07.004.
» https://doi.org/10.1016/j.cemconres.2005.07.004 -
[5] RASHID, S.A., AZIZ, F.N.A., SALEH, M.A.M., et al, “Investigations on the permeability properties development of binary blended concrete with nano-SiO2 particles”, Journal of Composite Materials, v. 45, n. 19, pp. 1931–1938, 2010. doi: http://doi.org/10.1177/0021998310389091.
» https://doi.org/10.1177/0021998310389091 -
[6] OH, T., CHUN, B., JANG, Y.S., et al, “Effect of nano-SiO2 on fiber-matrix bond in ultra-high-performance concrete as partial substitution of silica flour”, Cement and Concrete Composites, v. 138, pp. 104957, 2023. doi: http://doi.org/10.1016/j.cemconcomp.2023.104957.
» https://doi.org/10.1016/j.cemconcomp.2023.104957 -
[7] ZHANG, M.H., LI, H., “Pore structure and chloride permeability of concrete including nanoparticles for pavement”, Construction & Building Materials, v. 25, n. 2, pp. 608–616, 2011. doi: http://doi.org/10.1016/j.conbuildmat.2010.07.032.
» https://doi.org/10.1016/j.conbuildmat.2010.07.032 -
[8] CHELLATHURAI, B.R., RYMOND, N.M., “Durability evaluation of treated pineapple leaf biopolymer composites for enhanced eco-friendly mortar towards sustainability”, Biomass Conversion and Biorefinery, v. 14, n. 8, pp. 9897–9913, 2024. doi: http://doi.org/10.1007/s13399-024-05431-6.
» https://doi.org/10.1007/s13399-024-05431-6 -
[9] NAZARI, A., RIAHI, S., “The role of SiO2 nanoparticles and ground granulated blast furnace slag admixtures on physical, thermal and mechanical properties of self-compacting concrete”, Materials Science and Engineering A, v. 528, n. 4-5, pp. 2149–2157, 2011. doi: http://doi.org/10.1016/j.msea.2010.11.064.
» https://doi.org/10.1016/j.msea.2010.11.064 -
[10] ALY, M., HASHMI, M.S.J., OLABI, A.G., et al, “Effect of colloidal nano-silica on the mechanical and physical behaviour of waste-glass cement mortar”, Materials & Design, v. 33, pp. 127–135, 2012. doi: http://doi.org/10.1016/j.matdes.2011.07.008.
» https://doi.org/10.1016/j.matdes.2011.07.008 -
[11] HEIDARI, A., TAVAKOLI, D., “A study of the mechanical properties of grinded ceramic powder concrete incorporating nano-SiO2 particles”, Construction & Building Materials, v. 38, pp. 255–264, 2013. doi: http://doi.org/10.1016/j.conbuildmat.2012.07.110.
» https://doi.org/10.1016/j.conbuildmat.2012.07.110 -
[12] HOSSEINI, P., BOOSHEHRIAN, A., DELKASH, M., et al “Use of nano-SiO2 to increase microstructure and compressive strength of recycled aggregate concretes”, In: Bittnar, Z., Bartos, P.J.M., Němeček, J. (eds), Nanotechnology in construction, Springer, Berlin, pp. 215–221, 2009. doi: http://doi.org/10.1007/978-3-642-00980-8_29.
» https://doi.org/10.1007/978-3-642-00980-8_29 -
[13] SOLTANIAN, H., ARDJMANDA, M., YADEGARI, A., et al, “The effect of nanosilica on the physical properties of oil well cement”, Materials Science and Engineering, v. 538, pp. 288–294, 2012. doi: http://doi.org/10.1016/j.msea.2012.01.045.
» https://doi.org/10.1016/j.msea.2012.01.045 -
[14] SINGH, L.P., AGARWAL, S.K., BHATTACHARYYA, S.K., et al, “Preparation of silica nanoparticles and its positive effect in cementitious materials”, Nanomaterials and Nanotechnology, v. 1, n. 1, pp. 44–51, 2011. doi: http://doi.org/10.5772/50950.
» https://doi.org/10.5772/50950 -
[15] SINGH, L.P., BHATTACHARYYA, S.K., SINGH, P., “Granulometric production and characterization of dispersed nano silica powder and its use in the cementitious system”, Journal of the European Ceramic Society, v. 32, pp. 220–227, 2012. doi: http://doi.org/10.1179/1743676112Y.0000000002.
» https://doi.org/10.1179/1743676112Y.0000000002 -
[16] JO, B.W., KIM, C.H., TAE, G., et al, “Characteristics of cement mortar containing nano-SiO2 particles”, Construction & Building Materials, v. 21, n. 6, pp. 1351–1355, 2007. doi: http://doi.org/10.1016/j.conbuildmat.2005.12.020.
» https://doi.org/10.1016/j.conbuildmat.2005.12.020 -
[17] STEFANIDOU, M., PAPAYIANNI, I., “Nano-effect of SiO2 on Portland cement pastes”, Composites. Part B, Engineering, v. 43, n. 6, pp. 2706–2710, 2012. doi: http://doi.org/10.1016/j.compositesb.2011.12.015.
» https://doi.org/10.1016/j.compositesb.2011.12.015 -
[18] SANCHEZ, F., SOBOLEV, K., “Nanotechnology in concrete: a review”, Construction & Building Materials, v. 24, n. 11, pp. 2060–2071, 2010. doi: http://doi.org/10.1016/j.conbuildmat.2010.03.014.
» https://doi.org/10.1016/j.conbuildmat.2010.03.014 -
[19] LIN, D.F., LIN, K.L., CHANG, W., LUO, H., et al, “Improvements of nano-SiO2 on sludge/fly ash mortar”, Waste Management, v. 28, n. 6, pp. 1081–1087, 2008. doi: http://doi.org/10.1016/j.wasman.2007.03.023. PMID:17512717.
» https://doi.org/10.1016/j.wasman.2007.03.023 - [20] CHOWDHURY, R., ISLAM, M.S., RAHMAN, M., et al, “Pineapple leaf fibre reinforced engineered cementitious composites: a review”, SN Applied Sciences, v. 7, pp. 186, 2025.
-
[21] SILVA, J.M., ARRUDA FILHO, A.B., FARIAS, L.N., et al, “Characterization and application of different types of pineapple leaf fibers (PALF) in cement-based composites”, Fibers, v. 13, n. 5, pp. 51, 2025. doi: http://doi.org/10.3390/fib13050051.
» https://doi.org/10.3390/fib13050051 - [22] SAJITH, V., RAJAN, S.S., ANITHA, R., “Sustainability potential of pineapple leaf fiber as reinforcement in green concrete”, Construction & Building Materials, v. 400, pp. 133008, 2023.