ABSTRACT
Since the mid-1970s, geopolymer mortars and concretes have been produced through the alkaline activation of mixtures containing natural raw materials or wastes rich in silica (SiO2) and alumina (Al2O3), using a two-part processing method. In general, these inorganic polymers exhibit good mechanical performance, thermal resistance, and tribochemical properties. The literature has demonstrated that mining tailings (dust) from slate dams rich in aluminosilicates can be reused to obtain geopolymer composites through alkaline activation with potassium hydroxide (KOH) or sodium hydroxide (NaOH), or even with other basic aqueous solutions such as sodium silicates. Currently, there is an attempt in the literature to improve the synthesis of geopolymer compounds by acid activation, called silicoaluminophosphates, among the various aqueous phosphate solutions and others described in the literature. Therefore, food-grade phosphoric acid (H3PO4) at a concentration of 85% was selected for this exploratory study. The scope of this research was to evaluate the potential use of slate mining residue as a raw material in the synthesis of geopolymer composites using the two-part method for civil construction applications, such as mortars for the manufacture of auxiliary lightweight paving structures, masonry enclosures, and auxiliary urban elements. The raw material was optimized by grinding in a ball mill for periods of 15 minutes, 2 hours, and 7 hours, until reaching the desired particle size for geopolymerization. The materials were subjected to laser particle size analysis and physicochemical characterization by XRF, XRD, and SEM of both the raw material and the geopolymer specimens (PCs). During the processing of the PCs, the setting time was analyzed, and then their mechanical behavior was evaluated by compression tests at 28 days. The results of the mechanical compressive strength were satisfactory, showing increases in the alkaline mixture mixes (1 and 2), with corresponding values of 100% and 47.33%, respectively. In the acidic mixture, in mixes (1 and 3), strength reached increases of 91% and 93%, indicating potential for application in non-structural masonry. It was concluded that slate residue can be applied in infrastructure, urban sanitation, paving of public roads, and auxiliary paving structures, using geopolymerization techniques.
Keywords:
Geopolymeric cements; Slate mining waste; Acid (silicoaluminophosphate); Basic activation
1. INTRODUCTION
The term “geopolymer,” coined by French scientist Joseph Davidovits in the 1970s, refers to a class of inorganic materials formed by activating silica- and alumina-rich precursors with alkaline solutions, producing a three-dimensional polymeric structure of aluminosilicates with high mechanical strength, chemical stability, and durability [1]. The resulting structure consists of Si and Al tetrahedrons interconnected by oxygen bridges, forming a stable covalent network. Although alkaline-activated systems (AAS) are the most widely investigated, there is also growing interest in geopolymers derived from acid activation, such as silicoaluminophosphates (SAP), which have inferior dielectric properties and high thermal stability [2,3,4].
Among the main advantages of geopolymers over conventional Portland cement are a reduction of up to 80% in CO2 emissions [5], greater resistance to chemical corrosion, low shrinkage, thermal stability, and resistance to freezing and thawing. Portland cement production is associated with environmental impacts due to the burning of fossil fuels and the thermal decomposition of limestone, which releases approximately 0.53 t of CO2 per ton of clinker [6], geopolymers require only an aluminosilicate precursor and an activator (alkaline or acid), which allows for more sustainable alternatives.
In this context, Life Cycle Assessment (LCA) emerges as a necessary tool to comprehensively measure the environmental impacts associated with the production of geopolymer concretes. This study [7] represents one of the most comprehensive LCA analyses in this field. The authors incorporated all stages of the production process, from the extraction and transportation of raw materials to the production and application of concrete, also including the energy consumption and emissions associated with the manufacture of alkaline activators, such as sodium hydroxide (NaOH) and sodium silicate (Na2SiO3). Studies indicate that, by disregarding the environmental effects of activators, analyses may associate the benefits of geopolymers with Portland cement [2]. Thus, the importance of integrated LCA approaches that jointly consider the type of precursor, the activator used, and the curing process is highlighted.
In life cycle analysis (LCA) studies, geopolymers can reduce CO2 emissions by between 26% and 45% compared to Portland cement, depending on the formulation and energy source used [8]. Furthermore, the thermal curing step (60–80°C for 24 h) can represent approximately 12.4% of total emissions, equivalent to approximately 40 kg CO2e/m3, [7] a factor little considered in the literature [7]. Geopolymers cured at room temperatures offer environmental and economic advantages. According to the authors, [9] ambient curing reduces energy consumption and CO2 emissions, although it requires longer curing times to achieve optimal mechanical strength. Therefore, industrial activators and the use of heat increase emissions associated with geopolymers. Adopting ambient curing can mitigate these impacts and make these materials more viable, economical, and environmentally sustainable.
They [10] proposed an innovative route for producing activators using agricultural waste (RHA) (rice husk ash) and industrial waste (glass powder – WGP) as sustainable alternatives to conventional industrial inputs. The sustainability analysis, based on embodied energy (EE) and embodied CO2 emissions (ECO2-e), revealed reductions of up to 63% in embodied energy and up to 80% in emissions compared to Portland cement. Furthermore, geopolymers formulated with these activators demonstrated adequate mechanical performance and durability, even when exposed to aggressive environments containing magnesium sulfate and sulfuric acid. Second, [11] they carried out a simplified LCA evaluation of one-part geopolymers Alkaline Activated Materials (AAMs) proposed replacing commercial sodium silicate with a solid activator obtained through thermal fusion between recycled soda-lime glass and NaOH. The analysis indicated that, although NaOH has a high carbon footprint (1200 kg CO2-e/t), its controlled proportion (48% of the activator mass) and the use of waste glass (emissions of only 50 kg CO2-e/t) resulted in formulations with reductions of up to 84% in total CO2-e emissions compared to Portland cement. The WGAP formulation (with glass as activator and precursor) demonstrated technical performance and was in line with the reference values established by [7]. Studies such as those by [3, 12, 13] demonstrate the potential of activators obtained from RHA, WG (soluble glass), and silica fume, demonstrating emission and energy reductions, as well as improved mechanical performance (exceeding 100 MPa in some cases). These alternative routes have proven effective for producing sodium silicate or “sodium water glass” without the need for conventional high-temperature melting, which increases the technical and environmental viability of geopolymers on an industrial scale.
The application of LCA to the analysis of geopolymer systems, combined with the use of waste materials such as slate dust and alternative activators with lower environmental impact, addresses a strategy for developing more sustainable cementitious materials. Incorporating industrial and mineral waste into binder formulations contributes not only to reducing CO2 emissions and energy consumption, but also to mitigating environmental liabilities and enhancing the value of local resources.
Although various studies have investigated the use of mineral tailings in geopolymer matrices, many have explored acid or alkaline activation of mining waste. For example, iron ore tailings were activated with phosphoric acid to synthesize phosphate geopolymers, achieving strengths compatible with construction applications [14]. Other studies have developed phosphate binders from a combination of tailings, ash, or metakaolin, evaluating their mechanical and microstructural properties [15, 16]. Recent reviews also highlight the growing interest in phosphate-activated geopolymers (PAPs), pointing out advantages and limitations compared to alkaline-activated routes [17]. Furthermore, studies with one-part formulations reinforce the importance of investigating different activation routes and processing conditions [18]. However, although recent research explores the use of slate cutting residues and sludge in alkaline-activated geopolymers, as in the studies [17, 19], no records were found in the literature of investigations employing acid activation with phosphoric acid (H3PO4) applied to slate, nor comparisons between acidic and alkaline routes for this precursor. This absence demonstrates a specific gap in the literature and reinforces the scientific and technological relevance of this research.
In this context, this work proposes the use of slate mining waste, a plentiful environmental liability in Minas Gerais, located in the cities of Martinho Campos and Papagaios, a region known as the “slate province” and responsible for approximately 90% of national production. Despite its availability, this waste remains underexploited as a geopolymer precursor. Unlike other mineral wastes already studied (such as iron ore tailings or fly ash), slate has a high Si/Al ratio (7:1), a characteristic that compromises the formation of aluminosilicate gel and limits its use in structural applications. To our knowledge, there are no records of studies comparing slate in acidic and alkaline curing processes under ambient conditions, correlating microstructural properties, mechanical performance, and sustainability aspects, demonstrating a specific gap in the literature. The scientific contribution of this study is to demonstrate, in an innovative way, how the high Si/Al ratio of slate influences geopolymerization efficiency and the formation of phosphate and aluminosilicate phases aspects still little explored in naturally occurring low-reactivity waste. Methodologically, the research adopts an integrated approach that combines microstructure analyses (SEM, EDS, and XRD), mechanical performance, and sustainability assessment (LCA), offering a comparative and comprehensive view of the activation mechanisms a perspective rarely addressed in similar studies. The practical contribution lies in the use of a regional environmental liability slate mining waste from Minas Gerais promoting its local valorization and contributing to the reduction of environmental impacts and the strengthening of the circular economy, with potential for application in non-structural materials and sustainable construction elements. Thus, the originality of this study lies in: (i) investigating slate as a geopolymer precursor, highlighting its chemical composition and regional relevance; (ii) to compare in a structured manner two distinct activation routes (acidic with H3PO4 and alkaline with Na2SiO3 + KOH); (iii) to integrate analyses of microstructure, reaction products, mechanical strength, and sustainability indicators; and (iv) to discuss the viability of the material in non-structural applications, aligned with the circular economy and the valorization of local liabilities. Thus, the work presents an innovative contribution by proposing a valorization route for an abundant and still little explored mining residue, distinct from the most common approaches reported in the literature [17, 19] expanding the scope of alternative raw materials to produce eco-efficient binders.
2. MATERIALS AND METHODS
Chemical analysis of the slate powder was conducted using a Hitachi TM 4000 II benchtop scanning electron microscope (SEM). Samples were prepared in sample holders coated with TF-250 polypropylene film and analyzed in a vacuum atmosphere to identify and quantify the oxides present. The slate powder was then dried in a muffle furnace at 105°C for 8 h and ground in a Bond SL-36/21, 740 W, ore mill with 98 steel balls. Grinding was carried out with the slate powder completely dry and free of moisture for periods of 15 minutes, 2 hours, and 7 hours, at an average rotation speed of 60 rpm.
This step aimed to promote successive collision of the spheres, which progressively breaks down the material, reducing it to smaller particles before undergoing the geopolymerization reaction. After grinding, particle size was assessed by wet sieving through a 75 μm sieve, resulting in 99% passing material. Subsequently, a laser diffraction test was performed on a CILAS 1090® equipment in an aqueous medium, using ultrasound for 60 seconds, Fraunhofer model, to measure the particle size distribution of the slate powder residue, obtaining an obscurity value of approximately 13%. Grinding times of 15 minutes, 2 hours, and 7 hours resulted in average particle sizes of 9.75 μm, 8.24 μm, and 5.4 μm, respectively.
The results showed that the slate powder residue is considered fine compared to Portland cement. The average diameter (dM) obtained plays a key role in improving the cementitious matrix, since, in the production of geopolymer materials, it is desirable that most particles have dimensions smaller than 65 μm [20, 21]. This occurs because reducing particle size results in an increase in specific surface area, favoring the material’s reactivity and improving the geopolymerization process. To determine the initial and final setting times, the guidelines of the standard [22] for Portland cement paste were followed. The test was conducted on samples of alkaline and acidic mixtures at room temperature (approximately 25°C). Measurements were taken every 10 minutes to identify two characteristic points of changes in the paste’s rheology: the first (T1), indicating stiffening with increasing viscosity, and the second (T2), marking the transition from the plastic to the solid state [23].
The geopolymerization reaction and formation of the tetrahedral network were alkaline sodium silicate type C-122, with 14.8% Na2O (supplied by Inovações Ltda.), residual potassium hydroxide (KOH) solution (produced by Katrium Indústria Química Ltda. and supplied by Inovações Ltda.), and food-grade phosphoric acid (H3PO4) with a concentration of 85% (supplied by Inovações Ltda.). The choice of phosphoric acid with a purity of 85% is justified by its availability in the national market and its safe handling, important characteristics in exploratory studies aimed at demonstrating technical-scientific feasibility. This practice is addressed in research on acidic geopolymers, such as those of [2, 3] who employed concentrated H3PO4 to investigate the formation of silicoaluminophosphates (SAPs) with good mechanical and structural performance [24, 25]. Studies such as those of [4, 26] also highlight that the use of concentrated phosphoric acid is essential for the formation of Al–O–P and Si–O–P polymer networks, in addition to reducing curing time and favoring the formation of phases such as AlPO4 (berlinite), with initial strength gains [27]. Despite the high cost of the food-grade reagent, its use in this work aimed to ensure reproducibility and reliability of the results. For future industrial-scale applications, more economical alternatives are being investigated, such as the use of technical phosphoric acid or the recovery of phosphates from industrial effluents. In the alkaline activation process, geopolymer mortars with dimensions of 2.5 × 5 cm were manufactured in three different mixes, keeping the precursor proportions constant and varying the concentrations of the activator’s sodium silicate and potassium hydroxide. The alkalinity levels used were high (19.27%) for mix 1, intermediate (4.89%) for mix 2 and low (0.76%) for mix 3, expressed as a percentage w/w. Mechanical analyses were performed in five replicates (n = 30) for the alkaline mixture and in four replicates (n = 12) for the acidic mixture. Mean values and standard deviations were obtained for experimental monitoring, with a 68% confidence interval (i.e., one standard deviation for each side of the mean of the sampling distribution). Table 1 presents the proportions for two-part alkaline activation.
Dry mix proportions (m/m) for geopolymer blends produced by alkaline activation at room temperature curing (approximately 27 °C) for 12 h.
This study evaluated three concentrations of alkaline (Na2O and KOH) and acidic (H3PO4) activators on the performance of geopolymer mortars formulated from slate powder, with the aim of understanding the effect of these parameters on the reactivity and final properties of the aim of understanding the effect of these parameters on the reactivity and final properties of the material. The concentrations were selected based on ranges adopted in the literature for precursors rich in aluminosilicates, as proposed by [2, 3, 28].
For alkaline activation, concentrations of 0.76%, 4.89% and 19.27% m/m were used, based on the molar proportions recommended by [27]. For acid activation, concentrations of 14.87%, 26.16% and 29.84% m/m were used, according to studies by [2,3,4]. Preliminary tests indicated that these ranges provided workability, stability and reproducibility of the mixtures.
The geopolymerization process was favored by the dissociation of the alkaline activators into OH− ions and Na+ or K+ cations, with the hydroxyl responsible for catalyzing the reaction and the cations for stabilizing the charge of the formed structure [29]. The addition of silicates to the mixed activators also contributed to the increase in the nucleation rate, as reported by [30, 31]. The choice of three concentration levels for each type of activator, in an exploratory approach, allowed comparing their effects on the mechanical performance of the samples, which are important to guide future optimizations in the formulation of geopolymers with precursors in mineral waste.
The mixtures were prepared with a solid phase (slate powder) and a liquid phase (Na2O and KOH solutions) diluted in water. Homogenization was performed in a kitchen mixer for 20 minutes, resulting in pastes with a consistency similar to that of dry concrete. For the acidic mixtures, cylindrical specimens (2.5 × 5 cm) were molded with the three H3PO4 concentrations as shown in Table 2.
Proposed mixing ratios for geopolymer blends (w/w) produced by acid activation with ambient curing temperature for (approximately 27ºC) for 12 h.
The materials were weighed with a precision analytical balance, mixed, and compacted to avoid voids and bubbles. Curing was carried out at room temperature (approximately 27°C) for 12 hours, covered with glass plates for 24 hours to prevent carbonation. After demolding, the samples were stored in closed plastic boxes until testing, respecting the age at rupture as per the standard [32]. Similarly, the alkaline mixture specimens were molded to the same size as recommended by standard [32] and underwent the same curing and storage procedures. This careful preparation ensured that results could be compared between the different types and concentrations of activators.
3. RESULTS
After laser granulometry, the samples were analyzed by X-ray Fluorescence (XRF), presenting quantitative results with the presence of the following chemical elements, in order of occurrence: Si, Al, Fe, K, Ca, Ti, and Mn. The contents of the oxides present in the sample are presented in Table 3.
These results confirm literature data, demonstrating that the main constituents present in the slate dust residue are quartz, clinochlore, muscovite, albite, and orthoclase. Silica is the main constituent of the residue, representing approximately 60.66% of the sample by mass, followed by lower contents of alumina (aluminum oxide) (16.54%), iron oxide (13.63%), and K2O (5.26%). The sample composition presents a high concentration of silica and alumina, attributed to the presence of hydrated aluminosilicates in the slate.
Studies carried out by [33] present similar results in research focused on the development of porous slates. According to [34] their patent demonstrated the pozzolanic activity of slate and highlighted that the sum of the oxides SiO2, Al2O3, and Fe2O3 exceeds 70%. In this analysis, the sum of oxides was 90.83%, corroborating the values obtained in the present study. Thus, the X-ray Fluorescence (XRF) results indicate that the slate powder residue has a chemical composition suitable for use as a precursor in the formulation of mortars or geopolymer cements, since the mass ratio of silica and alumina was adequate. Although the formulation was estimated for a Si/Al molar ratio of 3:1, chemical analysis indicated an effective ratio of 7:1, due to the low aluminum content in the slate residue.
Table 4 presents the quantitative results for the oxides present. This disproportion, with a high silica-to-aluminum content, may limit its application in geopolymer concretes for structural purposes, as it is more suitable for non-structural or low-strength applications.
However, the literature reveals that Si/Al ratios greater than 5:1 tend to result in low compressive strength and a greater tendency to dissolve in water, making them unsuitable for structural applications in civil construction [35]. This study identified a Si/Al ratio of 7:1, which compromised the strength of geopolymer mortars, a behavior that is consistent with the literature. High Si/Al ratios favor the formation of longer, more open chains, leading to a structure with lower cross-link density and, consequently, lower structural integrity [36]. Generally, the recommended Si/Al molar ratio is between 1.5 and 3.5 for structural purposes, as values within this range favor the formation of a more cohesive three-dimensional network with higher cross-link density and better mechanical performance [1, 28, 37]. The molar ratio between SiO2/Na2O is estimated to be in the range of 0.12 to 3.0 [38].
To adapt the material to structural use, it would be necessary to reduce the Si/Al ratio to the recommended ideal range by adjusting the mix composition, for example, by increasing the alumina fraction by incorporating metakaolin or another Al-rich precursor, or by reducing the soluble silicate content in the activator. Furthermore, optimizations in curing time and activation temperature can also contribute to improving geopolymer network formation and increasing compressive strength [1, 26, 35]. Another parameter for optimizing the mechanical strength of geopolymers is the control of the molar ratios M2O/SiO2 and M2O/Al2O3, where M represents Na or K. According to the patent described by [39], it is recommended that the M2O/SiO2 ratio be in the range of 0.20 to 0.48, while the M2O/Al2O3 ratio should vary between 0.8 and 1.6. Increasing the concentration of M2O or reducing the amount of SiO2 in the activator solution has been associated with improved mechanical properties of geopolymers [40,41,42,43,44]. On the other hand, excess silicate can compromise the formation of the polymer network, inhibiting polymerization and intensifying water evaporation during curing, which reduces structural cohesion [1, 27].
Figure 1 presents the X-ray diffraction (XRD) results of the slate powder residue. Using the PDF databases of the International Centre for Diffraction Data (ICDD), the following crystalline phases were identified: quartz (Q) – SiO2, clinochlore (C) – (Mg,Fe2+)5Al(Si3Al)O10(OH)8, muscovite (M) – KAl2(AlSi3O10)(OH)2, albite (A) – NaAlSi3O8, and orthoclase (O) – KAlSi3O8. Muscovite is a hydrated potassium aluminum silicate, belonging to the mica class; clinochlore is a hydrated silicate of magnesium, iron, and aluminum, belonging to the chlorite group and responsible for the green color of schists and slates; albite is a sodium silicate belonging to the plagioclase feldspar series; and orthoclase is a potassium silicate belonging to the alkali feldspar group [45,46,47]. These results confirm the presence of the main minerals found in slate, as described in the literature.
Table 5 shows the start and end times for alkaline and acidic samples using the Vicat method. The tests were conducted at an ambient temperature of approximately 26 °C.
As shown in Table 5, the values obtained indicated a workability time of more than 2 h 50 min. Although this time is longer than that observed for Portland cement mortar (60–120 min), according to [22], it is compatible with phosphoric acid-activated geopolymers, especially when using low-reactivity aluminosilicates, such as slate residue, and when curing occurs at room temperature [2, 3]. Although it limits its use in applications requiring rapid hardening, this characteristic favors specific uses, such as sealing panels, non-structural precast elements, masonry mortars, and urban elements, as suggested by [4, 28]. Furthermore, extended handling time can be advantageous in industrial or artisanal applications that require detailed molding or laying at high temperatures [2, 30]. Nevertheless, to expand the applicability of these mortars, the use of additives that adjust setting time according to the application requirements can be considered.
Figure 2(a)–(c) show micrographs obtained by scanning electron microscopy (SEM) of geopolymers synthesized with different concentrations of alkaline activators. Figure 2(a) shows the sample with a concentration of 0.76%, exhibiting a porous and heterogeneous matrix, with angular particles and unreacted slate powder. As the alkali concentration increased to 4.89% (Figure 2(b)), a partially homogeneous structure was observed, with lower porosity and the initiation of gel formation. The sample with 19.27% activator (Figure 2(c)) presented a dense and homogeneous matrix, with spherical structures characteristic of N-A-S-H gel formation, in addition to a more cohesive and resistant matrix [29, 31]. These results agree with the compressive strength tests, indicating a correlation between the developed microstructure and the mechanical performance of the geopolymer mortars.
Energy Dispersive Spectroscopy (EDS) results indicated that geopolymer mortars with 4.89% and 19.27% alkaline solutions had higher Al/Si ratios compared to those with 0.76%. According to the geopolymer synthesis reaction [29], these reactions are fundamental for strength development and are controlled by the Al/Si and Na/Al ratios. In compositions with low calcium content, such as fly ash or similar residues, the amorphous N-A-S-H gel is the main reaction product, responsible for mechanical strength [31]. Furthermore, according to [29], the use of potassium hydroxide (KOH) can reduce efflorescence formation because its bonds with the aluminosilicate gel are stronger, and potassium carbonate crystals tend to be less visible than those formed by sodium. According to [33], efflorescence was also reduced in geopolymers cured between 25°C and 80°C.
In the present study, the samples with the highest Al/Si ratios were those prepared with 4.89% and 19.27% alkaline solutions, which contributed to higher compressive strength. On the other hand, the lower concentration (0.76%) resulted in lower polymerization and compressive strength due to the insufficient amount of KOH and Na2SiO3 to promote the effective dissolution of Al ions. Furthermore, it was observed that the mortars with 19.27% activators presented the highest Na/Si ratios among all the formulations analyzed.
Figure 3(a)–(c) show micrographs of the geopolymers obtained with acid activation, in which it can be observed that the slate powder particles have a subtly rounded and spherical morphology, with small particles agglomerated on the surface of larger grains. This behavior can be attributed to the surface energy generated during material processing (grinding or firing), since curing occurred at an ambient temperature of approximately 27°C [48]. Furthermore, the presence of crystalline phases such as AlPO4, formed by the reaction between leached aluminum ions and PO43− anions, is observed. At the end of the curing process (between 16 and 21 days at room temperature), a geopolymer composite with a complex structure is obtained, composed of silica gel and Al–O–P and Si–O–T networks, in which T can represent Al, Si, or P units [49,50,51,52].
The compressive strength test results for the alkaline and acidic mixture samples are presented in Tables 6 and 7, respectively. The curve-fitting plots for these samples are shown in Figures 4 and 5.
Average values and standard deviations of compressive strength obtained for each alkaline sample in the compression test.
Mean values and standard deviations of compressive strength obtained for each acid sample in the compression test.
Variation of compressive strength as a function of the concentration of alkaline activators.
The experimental results demonstrated that increasing the alkali concentration promotes greater compressive strength in geopolymers, with emphasis on the mix with 19.27% alkali solution, which reached 2.81 MPa and a Si/Al molar ratio of 2.61. The mixes, with 4.89% and 0.76%, presented lower strengths (1.33 MPa and 0.35 MPa, respectively), with similar Si/Al ratios (2.56 and 2.55). These results showed that higher alkali concentrations not only intensify the geopolymerization reaction but also contribute to the formation of a denser and more cohesive three-dimensional network. Studies indicate that the mechanical strength of geopolymers is related to the Si/Al molar ratio and the efficiency of matrix polymerization [38, 40]. Second, [28, 41] geopolymers activated with NaOH and Na2SiO3 exhibit better mechanical performance when the Si/Al ratio is adjusted to 4.0. Furthermore, a higher Si/Al ratio tends to generate denser structures, resulting in better mechanical performance. According to [31, 53] state that increasing this ratio promotes more efficient polymerization of the geopolymer matrix. As with cementitious mortars, a smaller amount of aqueous phase favors the hardening of the geopolymer matrix, as it reduces the formation of excessive porosity. However, it is important to maintain an adequate proportion of alkaline activator solution to ensure efficient dissolution of the aluminosilicate precursors and allow the complete geopolymerization reaction [38]. These data suggest the existence of critical limits for both the Si/Al ratio and the alkali concentration, below which activation is insufficient to generate a cohesive structure, thereby impacting the mechanical properties of the material.
The data in Table 7 demonstrate that the acid-activated samples presented higher standard deviations ranging from 0.64 to 1.51 MPa, higher than those observed in the alkaline formulations (Table 6). This difference can be attributed to the complexity of acid geopolymerization mechanisms, which are less understood and influenced by parameters such as temperature, curing time, water/activator ratio, and phosphorus content [2]. Although high concentrations of phosphoric acid accelerate precursor dissolution, they can impair the formation of stable three-dimensional networks, resulting in brittle and porous structures [3].
In this study, all formulations with phosphoric acid presented a constant Si/Al molar ratio of 5.94. However, there was variation in compressive strength, influenced by the activator concentration. The highest strength, ranging from 1.51 to 4.68 MPa, was obtained with an intermediate concentration, followed by formulations with higher and lower acid contents, indicating nonlinear behavior. This trend, also reinforced by a second order polynomial curve (Figure 4), suggests the existence of an ideal phosphoric acid content that favors the formation of a denser and stronger matrix [54]. Previous studies also indicate that, although phosphoric acid acts in the dissolution and stabilization of aluminum, imbalances in the Si/P ratio, whether due to excess PO43− or incomplete dissolution of aluminosilicates, compromise structural integrity and reduce compressive strength [4, 49,50,51,52].
In an acidic environment, the greater reactivity of aluminum can favor the formation of rigid bonds, but excessive concentrations can destabilize the matrix [17, 55,56,57].
X-ray fluorescence (XRF) analysis, presented in Table 8, revealed variations in chemical composition according to the type of activator. In the acidic mixtures, P2O5 and K2O contents were observed, indicating the presence of phosphate phases. The alkaline formulations showed compositions typical of aluminosilicate-based systems. These differences impact the structure, reactivity, and mechanical properties of the geopolymers, as discussed by [27, 28, 58].
X-ray diffraction (XRD) analysis of the alkaline and acidic samples is shown in Figures 6 and 7. The following phases were identified in the alkaline sample: quartz (SiO2), clinochlore. (Mg,Fe²⁺)5Al(Si3Al)O10(OH)8, aluminum (Al2O3 hydrated sodium aluminum silicate), potassium (K2O) and calcium (CaO).
X-ray diffraction (XRD) analysis of the alkaline-activated geopolymer samples revealed a diffuse halo between 20° and 35° in 2θ, characteristic of the presence of an amorphous phase associated with the formation of a disorganized matrix of aluminosilicates. In addition, well-defined peaks corresponding to the crystalline phases of quartz, clinochlore, aluminum, potassium, and calcium were identified, indicating the presence of precursor minerals (slate powder) and partially unreacted secondary phases, such as C–S–H or N–A–S–H [24].
Aluminosilicate minerals, such as clinochlore, act as potential sources of silicon and aluminum, contributing to the formation of the geopolymers three-dimensional network. The presence of these partially unreacted phases is common in formulations with natural precursors rich in dissolution-resistant minerals, which can compromise the material’s mechanical strength and structural stability over time [24].
In Figure 7, the following phases were identified in the acid sample: quartz (SiO2), hydrated sodium aluminum silicate (Mg,Fe)5 Al(Si3 Al)O10 (OH)8 and calcium (CaO) potassium (K2O) and phosphorus (PO43−).
X-ray diffraction (XRD) analysis of the acid-activated samples confirms the presence of well-defined crystalline peaks and a diffuse halo between 20° and 35° (2θ), indicating the formation of crystalline and amorphous phases. The presence of the halo suggests the partial formation of an amorphous geopolymer matrix, while the peaks are associated with quartz, clinochlore, hydrated aluminum silicate, sodium, calcium, potassium, and phosphorus, revealing the incomplete incorporation of the precursor constituents (slate powder) [59]. This behavior is typical of systems formulated with natural precursors rich in low-solubility minerals, which, even under acid activation, tend to remain partially unreactive [50]. Despite this limitation, the evidence of phosphorus (P) and the possible presence of silicoaluminophosphate phases indicate that the activation reaction occurred, albeit with limitations regarding the dissolution and complete polymerization of the aluminosilicates. Furthermore, the presence of additional peaks may indicate the formation of semicrystalline or secondary phases, such as calcium hydrosilicates (C–S–H) and hydrated sodium and potassium [60] aluminosilicates (Na/C–A–S–H). The presence of minerals such as quartz indicates the existence of remaining unreacted phases, which may compromise the mechanical strength and thermal and chemical stability of the composite [55].
4. DISCUSSION
The characterization of the slate residue revealed silica (60.66%) and alumina (16.54%) contents, with the sum of SiO2, Al2O3 and Fe2O3 reaching 90.83%, a value compatible with pozzolanic materials, as presented by [21,22,23]. Although the composition is adequate, the high Si/Al mass ratio (7:1) exceeds the ideal range of 1.5 to 3.5 recommended for geopolymers with better mechanical performance [1, 28, 37] which compromises the structural integrity of the matrix. Compressive strength tests demonstrated that, in alkaline mixtures, increasing the activator concentration favored polymerization, particularly in the 19.27% mixture, which reached 2.81 MPa and a Si/Al ratio of 2.61. This behavior was confirmed by SEM and EDS analyses, which indicated greater formation of N–A–S–H gels at higher concentrations [53]. However, even with increasing the alkaline concentration, the values obtained were lower than expected for structural applications, highlighting the limitations of alkaline activation under ambient curing.
In the acidic formulations, the Si/Al ratio remained constant at 5.94, with the highest resistance observed at the intermediate concentration of phosphoric acid (4.68 MPa), suggesting an ideal activation point [54]. High acid concentrations did not result in greater strength, reinforcing the idea that structural stability is more closely linked to activator dosage than to raw material composition. Previous studies also indicate that excessive PO43− concentrations can compromise matrix cohesion due to uncontrolled aluminum dissolution [4, 55]. The presence of phosphate phases and Al–OP and Si–OT structures, confirmed by XRD, indicates the occurrence of the [57], geopolymerization reaction, albeit partial, given that part of the material remained crystalline [16, 50]. Setting times greater than 2 h 50 min, although long in relation to Portland cement, [22] are compatible with the use of low-reactivity precursors in acidic systems and may represent an advantage in applications that require greater workability [24]. Thus, the results indicate that slate residue has potential for use in non-structural applications, such as sealing blocks, precast elements, mortars, and urban infrastructure components. The main limitations of this study are the precursor’s low reactivity during ambient curing, the lack of heat treatments, and the use of a single type of residue, factors that limit mechanical performance. Future studies recommend incorporating aluminum-rich precursors, such as metakaolin, adjusting the molar ratios of the activators (M2O/SiO2 and M2O/Al2O3), applying controlled heat curing, and evaluating durability in aggressive environments, aiming to expand the applicability of the geopolymers produced. Table 9 presents comparisons between acidic and basic activations, based on the results obtained, highlighting differences in setting time, structure, stability, and suitability for different applications.
5. CONCLUSIONS
Therefore, it is concluded that phosphoric acid-activated slate residue presents better mechanical performance and greater stability under ambient curing conditions, while alkaline activation requires adjustments in molar ratios and the possible addition of complementary precursors to achieve high mechanical strength. Despite being an exploratory analysis, performed without additives, thermal curing, or formulation optimization, the results obtained were relevant. The future adoption of strategies such as the incorporation of fly ash, metakaolin, or other aluminosilicate-rich waste, as well as modifications in molar ratios and the application of thermal curing, may contribute to increasing the mechanical strength of composites. Future studies should also explore hybrid formulations and durability testing, aiming to expand the technical applicability of these materials. The use of slate residue contributes to the valorization of mineral liabilities and represents a viable alternative aligned with the circular economy, with potential application in coatings, sealing, lightweight paving, and other sustainable solutions in the construction industry [61, 28, 2].
By experimentally demonstrating and comparing acidic (H3PO4) and alkaline routes for slate residue under ambient curing, this work presents the extent to which searches conducted in indexed databases (Scopus) and recent reviews indicate [17, 19] an unprecedented valorization route for this regional asset. Thus, the research contributes in an integrated manner to the advancement of microstructural knowledge and the assessment of the sustainability of slate-derived geopolymer composites, providing a comparative basis that is still lacking in the literature and reinforcing the potential of these materials as sustainable, low-environmental-impact alternatives.
6. ACKNOWLEDGMENTS
The authors thank CAPES for the financial support provided during the completion of this work.
7. BIBLIOGRAPHY
-
[1] DUXSON, P., FERNÁNDEZ-JIMÉNEZ, A., PROVIS, J.L., et al., “Geopolymer technology: The current state of the art”, Journal of Materials Science, v. 42, n. 9, pp. 2917–2933, May. 2007. doi: https://doi.org/10.1007/s10853-006-0637-z.
» https://doi.org/10.1007/s10853-006-0637-z - [2] LIN, H., LIU, H., LI, Y., et al., “Properties and reaction mechanism of phosphoric acid activated me-takaolin geopolymer at varied curing temperatures”, Cement and Concrete Research, v. 144, n. 2, pp. 106425, 2021.
-
[3] TCHAKOUTÉ, H.K., RÜSCHER, C.H., “Mechanical and microstructural properties of metakaolin- based geopolymer cements from sodium waterglass and phosphoric acid solution as hardeners: A comparative study”, Applied Clay Science, v. 140, pp. 81–87, May. 2017. doi: https://doi.org/10.1016/j.clay. 2017.02.002.
» https://doi.org/10.1016/j.clay.2017.02.002 -
[4] ZHANG, B., GUO, H., DENG, L., et al., “Undehydrated kaolinite as materials for the preparation of geopolymer through phosphoric acid-activation”, Applied Clay Science, v. 199, pp. 105887, 2020. doi: https://doi.org/10.1016/j.clay.2020.105887.
» https://doi.org/10.1016/j.clay.2020.105887 -
[5] KRISHNA, R.S., MISHRA, J., NANDA, B., et al., “The role of graphene and its derivatives in modifying different phases of geopolymer composites: A review”, Construction & Building Materials, v. 306, pp. 124–774, Nov. 2021. doi: https://doi.org/10.1016/j.conbuildmat.2021.124774.
» https://doi.org/10.1016/j.conbuildmat.2021.124774 -
[6] DAMTOFT, J.S., LUKASIK, J., HERFORT, D., et al., “Sustainable development and climate change initiatives”, Cement and Concrete Research, v. 38, n. 2, pp. 115–127, Feb. 2008. doi: https://doi.org/10.1016/j.cemconres.2007.09.008.
» https://doi.org/10.1016/j.cemconres.2007.09.008 -
[7] TURNER, L.K., COLLINS, F.G., “Carbon dioxide equivalent (CO2-e) emissions”: A comparison between geopolymer and OPC cement concrete”, Construction & Building Materials, v. 43, pp. 125–130, Jun. 2013. doi: https://doi.org/10.1016/j.conbuildmat.2013.01.023.
» https://doi.org/10.1016/j.conbuildmat.2013.01.023 -
[8] RABIE, M., IRSHIDAT, M.R., AL-NUAIMI, N., “Ambient and heat-cured geopolymer composites: Mix design optimization and life cycle assessment”, Sustainability (Basel), v. 14, n. 9, pp. 4942, May 2022. doi: https://doi.org/10.3390/su14094942.
» https://doi.org/10.3390/su14094942 -
[9] WATTANACHAI, P., SUWAN, T. “Strength of geopolymer cement curing at ambient temperature by non-oven curing approaches: An overview”, IOP Conference Series: Materials Science and Engineering, v. 212, pp. 012014, May 2017. doi: https://doi.org/10.1088/1757-899X/212/1/012014.
» https://doi.org/10.1088/1757-899X/212/1/012014 -
[10] NASSAR, A.K., KATHIRVEL, P., MURALI, G., et al., “Innovative one-part Alkali activated binder from activator derived from agricultural waste: Synthesis and application for sustainable construction”, Results in Engineering, v. 21, pp. 101–975, Mar. 2024. doi: https://doi.org/10.1016/j.rineng.2024.101975.
» https://doi.org/10.1016/j.rineng.2024.101975 -
[11] SAMARAKOON, M.H., RANJITH, P.G., HUI DUAN, W., et al., “Extensive use of waste glass in one part alkali activated materials: Towards sustainable construction practices”, Waste Management, v. 130, pp. 1–11, Jun. 2021. doi: https://doi.org/10.1016/j.wasman.2021.04.060. PubMed PMID: 34044359.
» https://doi.org/10.1016/j.wasman.2021.04.060 -
[12] BERNAL, S.A., RODRÍGUEZ, E.D., DE GUTIÉRREZ, R.M., et al., “Performance at high temperature of alkali activated slag pastes produced with silica fume and rice husk ash-based activators”, Materiales de Construcción, v. 65, n. 318, pp. 1–10, Apr. 2015. doi: https://doi.org/10.3989/mc.2015.03114.
» https://doi.org/10.3989/mc.2015.03114 -
[13] RAJAN, H.S., KATHIRVEL, P., “Sustainable development of geopolymer binder using sodium silicate synthesized from agricultural waste”, Journal of Cleaner Production, v. 286, pp. 124–959, Mar. 2021. doi: https://doi.org/10.1016/j.jclepro.2020.124959.
» https://doi.org/10.1016/j.jclepro.2020.124959 - [14] CARVALHO, A.R., CALDERÓN-MORALES, B.R.S., BORBA JUNIOR, J.C., et al., “Proposition of geopolymers obtained through the acid activation of iron ore tailings with phos- phoric acid”, Construction & Building Materials, v. 403, n. 3, pp. 133078, Nov. 2023.
-
[15] TOME, S., BEWA, C.N., NANA, A., et al., “Structural and physico-mechanical investigations of mine tailing-calcined kaolinite based phosphate geo- polymer binder”, Silicon, v. 14, n. 7, pp. 3563–3570, May. 2021. doi: https://doi.org/10.1007/s12633-021-01137-w.
» https://doi.org/10.1007/s12633-021-01137-w - [16] BURDUHOS NERGIS, D.D., VIZUREANU, P., SANDU, A.V., et al., “Xrd and tg-dta study of new phosphate-based geopolymers with coal ash or metakaolin as aluminosilicate source and mine tailings addition”, Materials (Basel), v. 15, n. 1, pp. 202, Jan. 2022. PubMed PMID: 35009346.
-
[17] GORYUNOVA, K., GAHRAMANLI, Y., MURADKHANLI, V., et al., “Phosphate-activated geopolymers: advantages and application”, RSC Advances, v. 13, n. 43, pp. 30329–30345, Sep. 2023. doi: https://doi.org/10.1039/D3RA05131E. PubMed PMID: 37849710.
» https://doi.org/10.1039/D3RA05131E -
[18] PERUMAL, P., PIEKKARI, K., SREENIVASAN, H., et al., “One-part geopolymers from mining residues – Effect of thermal treatment on three different tailings”, Minerals Engineering, v. 144, pp. 106026, Sep. 2019. doi: https://doi.org/10.1016/j.mineng.2019.106026.
» https://doi.org/10.1016/j.mineng.2019.106026 -
[19] CARRILLO BELTRÁN, R., PICAZO CAMILO, E., PEREA TOLEDO, G., et al., “Towards a sustainable mining: Reuse of slate stone cutting sludges for new geopolymer binders”, Sustainability (Basel), v. 16, n. 8, pp. 3322, Apr. 2024. doi: https://doi.org/10.3390/su16083322.
» https://doi.org/10.3390/su16083322 -
[20] KOHOUT, J., KOUTNÍK, P., HÁJKOVÁ, P., et al., “Effect of aluminosilicates’ particle size distribution on the microstructural and mechanical properties of metakaolinit based geopolymers”, Materials (Basel), v. 16, n. 14, pp. 5008, Jul. 2023. doi: https://doi.org/10.3390/ma16145008. PubMed PMID: 37512282.
» https://doi.org/10.3390/ma16145008 -
[21] KAYA, K., SOYER-UZUN, S., “Evolution of structural characteristics and compressive strength in red mud metakaolin based geopolymer systems”, Ceramics International, v. 42, n. 6, pp. 7406–7413, May. 2016. doi: https://doi.org/10.1016/j.ceramint.2016.01.144.
» https://doi.org/10.1016/j.ceramint.2016.01.144 - [22] ASSOCIAÇÃO BRASILEIRA DE NORMAS TÉCNICAS, ABNT NBR 16607, Portland Cement Determination of Setting Times, Rio de Janeiro, ABNT, 2018.
-
[23] KOUTNÍK, P., SOUKUP, A., BEZUCHA, P., et al., “Low viscosity metakaolinite based geopolymer binders”, Construction & Building Materials, v. 230, pp. 116–978, Jan. 2020. doi: https://doi.org/10.1016/j.conbuildmat.2019.116978.
» https://doi.org/10.1016/j.conbuildmat.2019.116978 -
[24] DUXSON, P., PROVIS, J.L., LUKEY, G.C., et al., “The role of inorganic polymer technology in the development of ‘green concrete’”, Cement and Concrete Research, v. 37, n. 12, pp. 1590–1597, Dec. 2007. doi: https://doi.org/10.1016/j.cemconres.2007.08.018.
» https://doi.org/10.1016/j.cemconres.2007.08.018 -
[25] XU, H., VAN DEVENTER, J.S.J., “The effect of alkali metals on the formation of geopolymeric gels from alkali-feldspars”, Colloids and Surfaces. A, Physicochemical and Engineering Aspects, v. 216, n. 1–3, pp. 27–44, Apr. 2003. doi: https://doi.org/10.1016/S0927-7757(02)00499-5.
» https://doi.org/10.1016/S0927-7757(02)00499-5 -
[26] KONG, D.L.Y., SANJAYAN, J.G., “Effect of elevated temperatures on geopolymer paste, mortar and con- crete”, Cement and Concrete Research, v. 40, n. 2, pp. 334–339, Feb. 2010. doi: https://doi.org/10.1016/j.cemconres.2009.10.017.
» https://doi.org/10.1016/j.cemconres.2009.10.017 -
[27] XU, H., VAN DEVENTER, J.S.J., “The geopolymerization of alumino- silicate minerals”, International Journal of Mineral Processing, v. 59, n. 3, pp. 247–266, 2000. doi: https://doi.org/10.1016/S0301-7516(99)00074-5.
» https://doi.org/10.1016/S0301-7516(99)00074-5 -
[28] DUXSON, P.S.W.M., MALLICOAT, S.W., LUKEY, G.C., et al., “The effect of alkali and Si/Al ratio on the development of mechanical properties of metakaolin-based geopolymers”, Colloids and Surfaces. A, Physicochemical and Engineering Aspects, v. 292, n. 1, pp. 8–20, 2007. doi: https://doi.org/10.1016/j.colsurfa.2006.05.044.
» https://doi.org/10.1016/j.colsurfa.2006.05.044 -
[29] KHEDMATI, M., ALANAZI, H., KIM, Y.R., et al., “Effects of Na2O/SiO2 molar ratio on properties of aggregate-paste interphase in fly ash-based geopolymer mixtures through mul- tiscale measurements”, Construction & Building Materials, v. 191, pp. 564–574, Dec. 2018. doi: https://doi.org/10.1016/j.conbuildmat.2018.10.024.
» https://doi.org/10.1016/j.conbuildmat.2018.10.024 - [30] GONÇALVES, D.K.C., “Synthesis of geopolymer pastes based on phyllites”, Tese de D.Sc., Universidade Federal de Ouro Preto, Minas Gerais, Minas Gerais, 2022.
-
[31] SINGHI, B., LASKAR, A.I., AHMED, M.A., “Investigation on soil–geopolymer with slag, fly ash and their blending”, Arabian Journal for Science and Engineering, v. 41, n. 2, pp. 393–400, 2016. doi: https://doi.org/10.1007/s13369-015-1677-y.
» https://doi.org/10.1007/s13369-015-1677-y - [32] ASSOCIAÇÃO BRASILEIRA DE NORMAS TÉCNICAS, ABNT NBR 16697, Portland Cement Portland Requirements, Rio de Janeiro, ABNT, 2018
-
[33] CAMBRONERO, L.E.G., ROMAN, J.M.R., RUIZ-PRIETO, J.M., “Caracterización de espumas de pizarra con adiciones de cínquer de cemento”, Boletín de la Sociedad Española de Cerámica y Vidrio, v. 46, n. 2, pp. 86–90, 2007. doi: https://doi.org/10.3989/cyv.2007.v46.i2.254.
» https://doi.org/10.3989/cyv.2007.v46.i2.254 - [34] PIMENTA, F.T., Slate in Pozzolanic Cements Patent: PI1003671-7, Rio de Janeiro, National Institute of Industrial Patents, 2010. (In Portuguese).
- [35] PROVIS, J.L., VAN DEVENTER, J.S.J., Alkali activated materials, state of the art report rilem tc 224-aam, 1 ed., New York, Springer Dordrecht Heidelberg, 2013.
-
[36] SIYAL, A.A., MOHAMED, R.M.S.R., SHAMSUDDIN, R., et al., “A comprehensive review of synthesis kinetics and formation mechanism of geopolymers”, RSC Advances, v. 14, n. 1, pp. 446–462, 2024. doi: https://doi.org/10.1039/D3RA06205H. PubMed PMID: 38173565.
» https://doi.org/10.1039/D3RA06205H -
[37] ROVNANÍK, P., “Effect of curing temperature on the development of hard structure of metakaolin-based geopolymer”, Construction & Building Materials, v. 24, n. 7, pp. 1176–1183, Jul. 2010. doi: https://doi.org/10.1016/j.conbuildmat.2009.12.023.
» https://doi.org/10.1016/j.conbuildmat.2009.12.023 -
[38] PROVIS, J.L., LUKEY, G.C., VAN DEVENTER, J.S.J., “Do geopolymers actually contain nanocrystalline zeolites: A reexamination of existing results”, Chemistry of Materials, v. 17, n. 12, pp. 3075–3085, May. 2005. doi: https://doi.org/10.1021/cm050230i.
» https://doi.org/10.1021/cm050230i -
[39] WANG, H., LI, H., YAN, F., “Synthesis and mechanical properties of metakaolinite-based geopolymer”, Colloids and Surfaces. A, Physicochemical and Engineering Aspects, v. 268, n. 1–3, pp. 1–6, 2005. doi: https://doi.org/10.1016/j.colsurfa.2005.01.016.
» https://doi.org/10.1016/j.colsurfa.2005.01.016 -
[40] OZER, I., SOYER-UZUN, S., “Relations between the structural characteristics and compressive strength in metakaolin based geopolymers with different molar Si/Al ratios”, Ceramics International, v. 41, n. 8, pp. 10192–10198, 2015. doi: https://doi.org/10.1016/j.ceramint.2015.04.125.
» https://doi.org/10.1016/j.ceramint.2015.04.125 - [41] HARDJITO, D., RANGAN, B.V., Development and properties of low-calcium fly ash based geopolymer concrete, Perth, Curtin University of Technology, 2005.
- [42] DEER, W.A., FLEET, M.E., HOWIE, R.A., ZUSSMAN, J., Rock-forming minerals: Sheet silicates: Micas, 2 ed., v. 3, chapter 4, London, Longman, 1992.
- [43] DEER, W.A., HOWIE, R.A., ZUSSMAN, J., Rock-forming minerals: Framework silicates: Feldspars, 2 ed., v. 4a, chapter 4, London, Longman, 1992.
- [44] DEER, W.A., HOWIE, R.A., ZUSSMAN, J., Rock-forming minerals: Sheet silicates: Chlorites, 2 ed., v. 3b, chapter 2, London, Longman, 1992.
- [45] DEER, W.A., HOWIE, R.A., ZUSSMAN, J., Rock-forming minerals: Single chain: Silicates, 2 ed., v. 2, chapters 2, 3 and 4, London, Longman, 1992.
- [46] KLEIN, C., DUTROW, B., Handbook of materials science, 23 ed., New Mexico, Wiley, 2012.
-
[47] MINDAT MINERAL DATABASE, https://www.mindat.org, accessed in August, 2025.
» https://www.mindat.org -
[48] NAJAFI KANI, E., ALLAHVERDI, A., PROVIS, J.L., “Efflorescence control in geopolymer binders based on natural pozzolan”, Cement and Concrete Composites, v. 34, n. 1, pp. 25–33, Jan. 2012. doi: https://doi.org/10.1016/j.cemconcomp.2011.07.007.
» https://doi.org/10.1016/j.cemconcomp.2011.07.007 - [49] DA SILVA, M.C., RACANELLI, L.A., SOUZA, J.A.S., et al., “Study of the mechanical performance of geopolymer produced with high iron content”, Matéria (Rio de Janeiro), v. 28, n. 1, pp. e20220309, 2023.
-
[50] ZRIBI, M., SAMET, B., BAKLOUTI, S., “Mechanical, microstructural and structural investigation of phos- phate-based geopolymers with respect to P/Al molar ratio”, Journal of Solid State Chemistry, v. 281, pp. 121025, 2019. doi: https://doi.org/10.1016/j.jssc.2019.121025.
» https://doi.org/10.1016/j.jssc.2019.121025 -
[51] ZRIBI, M., SAMET, B., BAKLOUTI, S., “Effect of curing temperature on the synthesis, structure and me- chanical properties of phosphate-based geopolymers”, Journal of Non-Crystalline Solids, v. 511, pp. 62–67, May. 2019. doi: https://doi.org/10.1016/j.jnoncrysol.2019.01.032.
» https://doi.org/10.1016/j.jnoncrysol.2019.01.032 -
[52] LOUATI, S., BAKLOUTI, S., SAMET, B., “Acid based geopolymerization kinetics: Effect of clay particle size”, Applied Clay Science, v. 132-133, pp. 571–578, Nov. 2016. doi: https://doi.org/10.1016/j.clay.2016.08.007.
» https://doi.org/10.1016/j.clay.2016.08.007 - [53] DAVIDOVITS, J., “Geopolymer chemistry and sustainable development, The poly (sialate) terminology: a very useful anbd simple model for the promotion and understanding of green chemistry”, Conference: Ge- opolymer Green Chemistry and Sustainable Development Solutions, v. 1, pp. 9–17, 2005.
-
[54] CUI, X.M., LIU, L.P., HE, Y., et al., “A novel aluminosilicate geopolymer material with low dielectric loss”, Materials Chemistry and Physics, v. 130, n. 1–2, pp. 1–4, Oct. 2011. doi: https://doi.org/10.1016/j.matchemphys.2011.06.039.
» https://doi.org/10.1016/j.matchemphys.2011.06.039 -
[55] GAO, L., ZHENG, Y., TANG, Y., et al., “Effect of phosphoric acid content on the micro- structure and compressive strength of phosphoric acid-based metakaolin geopolymers”, Heliyon, v. 6, n. 4, pp. e03853, Apr. 2020. doi: https://doi.org/10.1016/j.heliyon.2020.e03853. PubMed PMID: 32373746.
» https://doi.org/10.1016/j.heliyon.2020.e03853 -
[56] WAN, Q., ZHANG, R., ZHANG, Y., “Structure and properties of phosphate based geopolymer synthesized with the spent fluid catalytic cracking (SFCC) catalyst”, Gels (Basel, Switzerland), v. 8, n. 2, pp. 130, Feb. 2022. doi: https://doi.org/10.3390/gels8020130. PubMed PMID: 35200511.
» https://doi.org/10.3390/gels8020130 -
[57] DJOBO, J.N.Y., MOUSTAPHA, N., NDJONNOU, L.P.T., et al., “The role of curing temperature and reactive aluminum species on characteristics of phosphate geopolymer”, RSC Advances, v. 12, n. 46, pp. 29653–29665, Oct. 2022. doi: https://doi.org/10.1039/D2RA04562A. PubMed PMID: 36321086.
» https://doi.org/10.1039/D2RA04562A - [58] PROVIS, J.L., VAN DEVENTER, J.S.J., Geopolymers: structure, processing, properties and industrial applications, Sawston, Woodhead Publishing, 2014.
-
[59] PICAZO CAMILO, E., VALENZUELA EXPÓSITO, J.J., CARRILLO BELTRÁN, R., et al., “Study of properties of novel geopolymers prepared with slate stone cutting sludge and activated with olive stone bottom ash”, Materials (Basel), v. 18, n. 8, pp. 8, 2025. doi: https://doi.org/10.3390/ma18081774. PubMed PMID: 40333398.
» https://doi.org/10.3390/ma18081774 -
[60] MABROUM, S., ABOULAYT, A., TAHA, Y., et al., “Elaboration of geopolymers based on clays by products from phosphate mines for construction applications”, Journal of Cleaner Production, v. 261, pp. 121317, Mar. 2020. doi: https://doi.org/10.1016/j.jclepro.2020.121317.
» https://doi.org/10.1016/j.jclepro.2020.121317 - [61] DAVIDOVITS J, “Geopolymer chemistry and sustainable development”, Conference: Geopolymer Green Chemistry and Sustainable Development Solutions, v. Session 1, pp. 9–17, Geopolymer Institute, Saint-Quentin, France, July 2005.