Open-access A physics-based model for surface roughness prediction in metal material extrusion incorporating deposition geometry and sintering shrinkage

ABSTRACT

This study proposes a physics-based model for predicting surface roughness in metal material extrusion using Inconel 625 composite filaments. The approach combines filament geometry, bonding-neck evolution, transient cooling, and sintering shrinkage to describe the transformation from the green-state surface to the final sintered morphology. The influence of build orientation was investigated through the thermal conditions governing inter-filament coalescence during deposition. Experimental validation was conducted for Upright, Edge, and Flat configurations, yielding average roughness values of 54.47 µm, 54.33 µm, and 27.37 µm, respectively. The predicted values were 53.0 µm, 53.0 µm, and 26.6 µm, with prediction errors below 3%. The results show that stronger convective cooling shortens the effective coalescence period, restricts bonding-neck growth, and increases surface roughness. In contrast, more stable thermal conditions promote smoother inter-filament fusion and lower roughness. The proposed framework provides a practical prediction tool for the investigated Inconel 625 MEX system and establishes a foundation for future validation under different material systems and processing conditions.

Keywords:
Metal MEX; Bonding neck; Theoretical model; Surface roughness modeling; Sintering shrinkage.

1. INTRODUCTION

Metal material extrusion (Metal MEX) has emerged as a cost-efficient route for fabricating metal components, particularly when complex geometries and material utilization are required [1,2,3,4,5]. In this process, a metal-polymer feedstock is deposited layer by layer and subsequently subjected to debinding and sintering to obtain a dense metallic part [6,7,8,9]. During deposition, the feedstock behaves as a viscoelastic filament, whereas after debinding and sintering it transforms into a consolidated metallic structure. Consequently, the final surface quality depends not only on the deposition stage but also on the dimensional changes occurring during debinding and sintering [2, 5, 8].

After extrusion, the filament is compressed into a flattened track that is commonly represented by an equivalent elliptical geometry in analytical models [10,11,12]. At the same time, neighboring filaments progressively develop an interfacial neck through viscous flow driven by surface tension, while the extent of this coalescence is limited by the available thermal window before solidification [13,14,15,16,17,18,19]. Consequently, the final surface profile is governed by the coupled effects of deposited geometry and time-dependent inter-filament coalescence.

Surface roughness depends strongly on build orientation, deposition strategy, and local thermal history [20,21,22,23,24]. Several analytical and experimental models have been developed to predict roughness in extrusion-based additive manufacturing [11, 12]. More recently, machine-learning approaches have also been applied to predict surface roughness and density in metal MEX from processing and geometrical parameters [25]. However, these formulations remain insufficient for metal MEX systems, because the part undergoes additional debinding, densification, and shrinkage before reaching its final form [6, 8, 26, 27]. Since filament geometry and interfacial valleys continue to evolve during sintering, roughness models developed for polymer extrusion cannot directly predict the final morphology of metal MEX parts.

The problem becomes more complex in metal MEX because the feedstock consists of a two-phase metal–polymer system [7, 9, 28, 29]. In addition, different build orientations produce distinct bonding configurations and heat dissipation conditions, leading to anisotropic surface morphologies [20, 30].

To address these issues, a physics-based roughness model is developed for metal material extrusion. The bonding-neck evolution is described through viscous-flow-driven coalescence under surface tension, while the available coalescence time is determined from the transient thermal condition during deposition [13, 16, 17].

The main novelty of this study lies not in simply extending existing FFF roughness models, but in developing a unified physics-based predictive framework specifically for metal MEX. Unlike previous analytical models developed for polymer FFF, which predict only the as-deposited surface morphology, the proposed framework establishes a direct physical link between the green-state geometry and the final surface roughness of the sintered part by coupling deposition geometry, bonding-neck evolution, transient thermal effects, and sintering-induced shrinkage. Consequently, the proposed model predicts the final surface roughness after sintering rather than only the roughness immediately after deposition. Experimental validation using Inconel 625 composite filaments fabricated in three different build orientations demonstrates good agreement between the predicted and measured roughness values.

The proposed framework focuses on the dominant physical mechanisms governing surface roughness evolution throughout the metal MEX process, rather than resolving local particle-scale phenomena. Accordingly, homogenized representations of geometry, material properties, and thermal behavior are adopted to capture the dominant process physics while preserving analytical tractability. This modeling strategy balances physical realism and analytical tractability and provides an appropriate first-order predictive framework for surface roughness.

2. MATERIALS AND METHODS

2.1. Material characteristics

In metal MEX technology, the filaments are often produced by mixing metal powders with polymer binders. Different kinds of metal filaments are available, including copper, brass, steel, aluminum, superalloys, and titanium. [30].

One of the most vital requirements is to ensure sufficient interlayer adhesion during fabrication to preserve the bond’s integrity after cooling. Other essential factors are selecting suitable feedstock materials, controlling effective temperature, and optimizing processing parameters, such as layer thickness and infill pattern. Advances in processing techniques and deeper insights into parameter-performance relationships will increase industrial adoption and reduce production costs [31, 32].

In metal MEX, the feedstock behaves as a viscoelastic composite during deposition and transforms into a metallic structure after debinding and sintering [33]. This multi-stage transformation fundamentally alters the surface formation mechanism, which cannot be captured by existing polymer-based models. The fabrication process of filaments for the metal MEX method consists of four main stages [7,8,9, 28, 29]. The first stage is mixing and binder preparation. Metal powders are thoroughly blended with a polymer binder system to ensure the homogeneous dispersion of metallic particles within the binder system. The metal powder typically accounts for approximately 60–70 vol.%, while the remaining 30–40 vol.% consists of thermoplastic polymers and additives. The polymers commonly used consist of polyethylene (PE), polyvinyl alcohol (PVA), and polyethylene glycol (PEG), due to the ease of melt and removal during the debinding stage. The second stage is extrusion, in which the composite feedstock is extruded through a heated die to form filaments with a fixed diameter, usually 1.75 or 2.85 mm. This step requires precise control of temperature, pressure, and extrusion speed to ensure that the filaments do not fracture, maintain suitable mechanical strength, and exhibit uniform diameters. Finally, in cooling and spooling, the filament is rapidly cooled after extrusion to preserve roundness and dimensional accuracy. The filaments are then wound onto spools for convenient use in 3D printing.

The metal MEX filament is a two-phase composite consisting of metal (m) and polymer (p). For each phase, the mass is mi, the volume is Vi, and the density is ρi. The volume fraction is expressed as:

(1) ϕ i = V i V c

and the mass fraction is expressed as:

(2) w i = m i m c

where the subscript c denotes composite filaments.

The mass fraction can also be expressed in terms of the density and volume fractions as follows:

(3) w i = m i m c = ρ i V i ∑ j ρ j V j = ρ i ϕ i ∑ j ρ j ϕ j = ρ i ϕ i ρ m ϕ + ρ p ( 1 − ϕ )

From this, the metal mass fraction w and volume fraction φ can be determined as follows:

(4) w = ρ m ϕ ρ m ϕ + ρ p ( 1 − ϕ ) ; ϕ = w ρ m w ρ m + 1 − w ρ p

The key physical properties of the filament are defined as follows:

Density:

(5) ρ g r e e n = ϕ ρ m + ( 1 − ϕ ) ρ p

Specific heat capacity:

(6) C g r e e n = w C m + ( 1 − w ) C p

The effective thermal conductivity of the composite filament was estimated using the Maxwell–Eucken model, a widely accepted homogenization approach for predicting the effective thermal conductivity of two-phase particulate composites [34]. Similar formulations have also been applied in additive manufacturing studies for evaluating the effective thermal conductivity of heterogeneous metallic materials [35]:

(7) k g r e e n = k p k m + 2 k p + 2 ϕ ( k m − k p ) k m + 2 k p + ϕ ( k m − k p )

where km and kp are the thermal conductivities of the metal powder and binder.

The effective thermal diffusivity of the composite filament can be expressed as:

(8) ε = k g r e e n ρ g r e e n C g r e e n

2.2. Geometrical representation of deposited filaments and shrinkage characterization

As illustrated in Figure 1, the deposited strand adopts a flattened geometry that can be represented using an equivalent elliptical profile for analytical modeling with semi-axes a and b.

Figure 1
Illustration of adhesion mechanism in the metal MEX process.

A Cartesian coordinate system (xoy) was defined based on the cross-section of the nth deposited layer, which was centered at its midpoint. The elliptical profile is expressed as:

(9) x 2 a 2 + y 2 b 2 = 1

where the semi-axes are determined as:

(10) a = E 2 ; b = l t 2

Here: E – Extrusion width; lt – Layer thickness; lt = lsintered /SR; lsintered – Post-Sintered layer height (mm).

The shrinkage can also be expressed as a retention ratio. The shrinkage ratio SR is defined as the ratio between the part volume after sintering and the volume immediately after printing:

(11) S R = S s i n t e r e d S g r e e n

where Sgreen – is the part volume in the as-printed state, typically provided by the manufacturer’s software, and Ssintered – is the volume after sintering, which can be approximated by the designed volume Ssintered ≈ Sdesign.

2.3. Surface roughness

Due to the circular geometry of the printing nozzle, the deposited strand adopts a flattened geometry governed by extrusion and gravity, resulting in an evolving contact interface between adjacent filaments. This effect becomes more significant in metal MEX, where the metal-binder mixture deforms under gravity and interlayer interactions during deposition. In principle, the surface roughness can be preliminarily related to process parameters and filament geometry [30, 31]. Figure 2 illustrates the typical surface morphology after printing. The key contribution of this study is the development of a unified predictive framework that links bonding-neck evolution in the green state to the final surface roughness after sintering. While previous works [31] focused mainly on experimental surface characterization and orientation effects, and sintering-induced dimensional changes were discussed separately in [8], these aspects have not been integrated into a single physics-based model. By coupling neck growth kinetics with a thermally defined coalescence time window and shrinkage transformation, the present model enables quantitative prediction of the final Rz from the green-state geometry under different build orientations.

Figure 2
Formation diagram of surface roughness after printing “green” part.

The height of the surface roughness Rzg can be calculated using the following formula [30]:

(12) R z g = R z p + Δ R z
(13) Δ R z = δ 2 + δ 3 + δ 4

where: Rzg is the average height of the total absolute values of the five highest peaks and the five deepest valleys of the profile within the standard evaluation length (L), after printing process; ΔRz – is the amount by which the actual height of the surface roughness exceeds the theoretically calculated value; δ2, δ3, δ4 – represent the components of surface roughness corresponding to the influence of printer nozzle size, size variations during the washing process, and size variations of the printing material during the sintering process, respectively; Rzp – the calculated theoretical height of surface roughness, after printing process; Rag is the average surface roughness of the green part.

Because the contribution of ΔRz is typically much smaller than Rzp that of, the total as-printed roughness can be approximated as follows:

(14) R z g = R z p

After printing, the parts are debound and sintered. During debinding, most of the wax and polymer binder is removed. Sintering consolidates the metal particles, reduces porosity, and induces dimensional changes, typically leading to densification and shrinkage [6, 26, 27].

In practice, densification is often incomplete, and some residual porosity may persist after sintering. Consistent with the homogenized analytical framework adopted in this study, uniform shrinkage is assumed to represent the overall densification behavior of the printed part.

Based on this assumption, the surface roughness of the final sintered part is given by:

(15) R z = S R ⋅ R z p

where Rz denotes the surface roughness of the sintered final part.

2.4. Thermal-controlled bonding neck evolution and surface roughness formation

2.4.1. Interfacial coalescence and geometrical evolution of deposited filaments

After printing, the theoretical surface roughness is denoted as Rzp. Due to the influence of gravity and the extrusion process, the cross-section of a deposited layer in MEX is approximated by an elliptical geometry [11, 12]. As illustrated in Figure 3, the deposited filament is approximated by an equivalent elliptical cross-section, with the local surface valley governed by the development of the bonding neck between neighboring filaments.

Figure 3
Surface roughness evolution from deposition to sintering in metal material extrusion.

Figure 4 illustrates the geometrical evolution of surface roughness during filament coalescence and sintering shrinkage in metal MEX. The deposited filaments are represented by equivalent elliptical profiles, while the final surface morphology is governed by the combined effects of inter-filament bonding, neck growth, and shrinkage-induced dimensional transformation. Depending on the relative arrangement of adjacent filaments, the surface profile may be controlled by both horizontal bonding between stacked layers and longitudinal bonding between neighboring filaments within the same layer.

Figure 4
Geometrical evolution of bonding-neck growth and surface roughness formation in metal MEX.

During the coalescence process, the material flow at the filament interface is driven by surface tension and follows a curved interfacial profile characterized by two local radii of curvature, r1 and r2, which evolve with the bonding angles θ and β. The geometrical parameters a and b denote the semi-major and semi-minor axes of the deposited elliptical filament, respectively. As bonding progresses, the interfacial neck expands and modifies the local valley depth between adjacent filaments, thereby reducing the theoretical roughness of the green-state surface Rzp. After debinding and sintering, additional densification and shrinkage further transform the surface profile, leading to the final roughness Rz of the sintered part.

The surface roughness Rz was determined as follows:

(16) R z = S R ( a − x ( θ f ) )

where x(θf) is the instantaneous radius of the bonding neck length

(17) x ( θ ) = r 1 s i n θ

when the coalescence process ceases, the half-contact angle between the two filaments is denoted as θf

According to the principle of volume conservation, at any given time t, the expression of the instantaneous radius r1 during the bonding process of the filaments is:

(18) r 1 = π r 0 π − θ + s i n θ c o s θ

where r0 is the radius of curvature of the ellipse, given by r0 = a2/b

The rate of change of the instantaneous angle θ is defined by the following differential equation [16, 17]:

(19) d θ d t = 2 Γ a ( π − θ + s i n θ c o s θ 3 π η b 2 ⋅ ( π − θ ) c o s 2 θ + s i n θ c o s θ ( π − θ ) 2 s i n 2 θ

where Γ is the surface tension (N/m) and η is the viscosity (Pa·s).

The time required for the material to solidify, from extrusion at the nozzle to the loss of viscoelasticity, is denoted as tc. When this critical time is reached, the bonding neck stops growing. From the Bellehumeur model [11], the transient temperature of the filament is expressed as:

(20) T ( t ) = T E + ( T L − T E ) e − m v t

when the temperature reaches the solidification threshold T(t) = Tg, the critical time tc can be obtained as:

(21) t c = − 1 m v l n ( T g − T E T L − T E )

where v is the nozzle travel velocity, Tg is the solidification temperature, TL is the melting temperature, TE is the ambient temperature, and m is the thermal coefficient, defined as:

(22) m = 1 + 4 α γ − 1 2 α

The coefficients α, γ are determined as follows:

(23) α = k ρ C ν ; γ h 1 P ρ C A ν

where k is the thermal conductivity (W/m.k), ρ is the density (kg/m3), C is the specific heat capacity (J/kg.K), v is the nozzle travel velocity (m/s), h1 is the convective heat transfer coefficient (W/m2.k), P is the perimeter of the filament cross-section (m), and A is the cross-sectional area of the filament (m2).

The above formulation demonstrates that the thermal coefficient m is strongly dependent on the convective heat transfer coefficient h1. As h1 increases, the parameter γ increases correspondingly, resulting in a larger value of m. Physically, this behavior reflects the enhancement of heat dissipation from the deposited strand and the acceleration of transient cooling.

When the bonding process ceases, the half-contact angle between the two filaments is denoted as θf, which is determined from the Bellehumeur model.

(24) ∫ 0 θ f d θ d θ / d t = t c

The final contact angle θf is obtained by integrating Eq. (19) with respect to time from t = 0 to t = tc, corresponding to the evolution of θ from 0 to θf.

Similar to the calculation of surface roughness in the case of stacked layers, the surface roughness when layers are placed side by side is determined as follows:

The surface roughness Rz is expressed as follows:

(25) R z = S R ( b − y ( β f ) )

where y(βf ) is the instantaneous radius of the longitudinal bonding neck length.

When the bonding process ceases, the half-contact angle between the two filaments is denoted as βf.

The relationship between the instantaneous radius r2, longitudinal bonding neck length 2y, and instantaneous angle 2β is:

(26) y ( β ) = r 2 s i n β

where:

(27) r 2 = π r 0 π − β + s i n β c o s β

The value of βf is determined by the same approach as used for θf.

2.4.2. Effect of convective heat transfer on transient filament cooling and bonding-neck evolution

The heat transfer process during deposition involves conductive heat transfer toward previously deposited layers and convective heat dissipation to the surrounding environment. Among these mechanisms, convective heat transfer plays a particularly important role because it directly determines the cooling rate of the deposited filament through the convective heat transfer coefficient h1. The convective heat flux from the exposed filament surface can be described according to Newton’s cooling law:

(28) q c o n v = h 1 A s ( T − T E )

where As is the exposed filament surface area; T is the instantaneous filament temperature.

Figure 5 illustrates the influence of the convective heat transfer coefficient h1 and build orientation on transient filament cooling, bonding-neck evolution, and theoretical surface roughness formation in metal MEX. In the upright orientation, the larger exposed surface area and longer thermal path promote stronger convective heat dissipation, resulting in faster cooling, shorter bonding time, smaller bonding-neck formation, and higher theoretical roughness Rzp. In contrast, the flat orientation exhibits weaker convective cooling and longer thermal retention, thereby enhancing inter-filament coalescence and reducing surface roughness. The edge orientation presents an intermediate thermal and geometrical behavior between the upright and flat configurations.

Figure 5
Effect of build orientation and convective heat transfer coefficient h1 on transient cooling, bonding-neck evolution, and theoretical surface roughness Rzp in metal material extrusion.

The heat dissipation rate increases proportionally with the convective heat transfer coefficient. Consequently, increasing h1 intensifies heat extraction from the deposited strand and accelerates filament cooling.

The influence of h1 becomes particularly significant under different build orientations because the exposed surface area and thermal dissipation conditions vary substantially with deposition geometry. In vertically oriented structures, the deposited filament possesses a larger exposed surface and a longer thermal path to the build platform. Consequently, local fluctuations in h1 generate non-uniform cooling rates and heterogeneous bonding-neck evolution across the deposited structure.

3. EXPERIMENTAL ANALYSIS

3.1. Experimental setup

To evaluate the accuracy of the proposed surface roughness model, three specimens were fabricated under identical processing conditions (Figure 6). Surface roughness was measured in directions perpendicular to both longitudinal and horizontal bonding necks. The material used in the metal MEX process was a composite filament consisting of Inconel 625 powder and a polymer binder [36]. The composition of the filament, based on the supplier’s data, is summarized in Table 1. It mainly consists of Inconel 625 alloying elements together with a polymer binder system. The metal powder exhibits a characteristic particle size of approximately 50 µm.

Figure 6
The size of the printed sample.
Table 1
Composition of the Inconel 625 filament.

The parameters used in the Bellehumeur-based model were treated as effective properties of the composite filament. Thermal properties were estimated using rule-of-mixture approaches, while rheological parameters were taken from the literature on highly filled feedstocks, where the binder phase governs the flow behavior [7, 8]. The processing temperatures, including extrusion and ambient conditions, were recorded directly during printing. The corresponding model parameters are listed in Table 2.

Table 2
Thermal Properties of Inconel 625 composite filament and the printing process.

The extrusion width E defines the width of a deposited filament and is a key geometrical parameter in the model. In the Markforged Metal X system, E is automatically determined by the Eiger software and treated as a process-dependent parameter reflecting the actual deposition behavior.

The CAD model data in STL format is managed online by the user via the supplier’s website, where model parameters such as the material, model size, and position on the printing bed can be configured. Additionally, the printing time and production cost of the model can be monitored and adjusted. All test specimens were printed under the same conditions and printing settings, as outlined in Table 3. Printing related parameters, including printed dimensions, print time, wash time, dry time, printed part mass, final part mass, and metal volume, are presented in Table 4. Based on these data, the shrinkage can be expressed as a retention ratio. The shrinkage ratio SR was derived from dimensional data provided by the Eiger system, which predicts both the printed and final geometries using calibrated material parameters specific to the Metal X system process. Accordingly, SR is defined as the ratio between the sintered and printed volumes. In this study, SR is treated as an effective process parameter representing the overall densification behavior during sintering.

Table 3
Printing parameters used for Inconel 625 samples in the material extrusion process.
Table 4
Effect of build orientation on dimensional transformation, shrinkage behavior, and mass evolution of Inconel 625 parts in material extrusion.

3.2. Surface roughness measurement

The specimens were fabricated in three common build orientations: Upright, Edge, and Flat. For each orientation, three independent samples were printed, and each sample was measured at three different locations, as shown in Figure 7.

Figure 7
Measurement orientations for surface roughness: a) Upright build orientation; b) Edge build orientation; c) Flat build orientation; (d) Filament paths and measurement directions.

Surface roughness measurements were conducted using a Keyence DSX1000 digital microscope (LMPLFLN50XBD objective, 720× magnification) in bright-field mode with 3D height extension, as shown in Figure 8. Roughness parameters were evaluated according to ISO 4287 using a Gaussian filter (ISO 16610), with an evaluation length of approximately 0.38 mm. The system was calibrated prior to measurement, and identical acquisition settings were maintained for all samples to ensure reproducibility.

Figure 8
Surface roughness measurement using the Keyence DSX1000 microscope.

In all cases, the measurement vector was selected perpendicular to the deposition path to characterize the staircase-like profile induced by the layer-by-layer extrusion mechanism.

For the Upright and Edge specimens Figures 7 a and b, the measurement direction was perpendicular to both the deposition path and the horizontal bonding necks.

For the Flat specimens Fig. 7c, the measurement direction was perpendicular to the deposition path, and the longitudinal bonding necks formed between parallel filaments within the same layer.

The surface roughness parameter Rz was defined as the mean value of nine measurements (three specimens × three positions), ensuring statistical representativeness and enabling direct comparisons between different build orientations.

4. RESULTS AND DISCUSSION

4.1. Shrinkage-induced evolution of inter-particle morphology and surface roughness

For each processing condition (printed, washed, and sintered), one representative specimen was examined by SEM, and images were collected from three different regions. Figure 9 presents the surface morphology at the printed, washed, and sintered states. The SEM observations reveal significant morphological evolution throughout processing, demonstrating that the final surface roughness in metal MEX is strongly influenced by shrinkage and densification during debinding and sintering.

Figure 9
SEM observations of inter-particle morphology evolution during the process.

In the printed condition, the metallic particles remained encapsulated by the polymer binder, forming a loosely packed structure with discontinuous contact regions and large inter-particle gaps. The characteristic particle dimensions measured from the SEM image were approximately 1.8–4.4 µm. After washing, partial binder removal promoted particle rearrangement and reduced the spacing between neighboring particles, producing a denser morphology with characteristic dimensions of approximately 2.40–5.6 µm.

More pronounced changes occurred after sintering. Diffusion-driven neck growth and isotropic shrinkage significantly reduced the residual surface defects, while the original particle boundaries became less distinguishable because of densification. Unlike the printed and washed conditions, the measured dimensions in the sintered structure mainly corresponded to residual pores, which decreased to approximately 0.60–1.60 µm. Compared with the printed condition, the characteristic defect size decreased by approximately 60–85%, indicating substantial smoothing of the deposited morphology during sintering.

These observations confirm that the final surface roughness in metal MEX is governed not only by deposited filament geometry, but also by shrinkage-induced morphological transformation during post-processing

4.2. Influence of build orientation on surface roughness formation

To facilitate reproduction of the proposed analytical model, a representative calculation for the Upright orientation is presented below. As an example, the predicted roughness for the Upright orientation was obtained by sequentially applying Eqs. (19)–(24). Using the parameters listed in Table 2, the critical coalescence time was calculated as tc = 3.115s, yielding a final contact angle of θf = 0.2886 rad. The corresponding bonding-neck size was x(θf) = 0.1279 mm. Substituting a = 0.22 mm, x(θf) = 0.1279 mm, and the shrinkage coefficient SR = 0.579 into Eq. (16) gives Rz ≈ 53 μm. The same calculation procedure was applied to the other build orientations.

The predicted and measured surface roughness of metal MEX samples are detailed in Table 5.

Table 5
Surface roughness (Rz, µm) according to build orientation and bonding type.

Upright and Edge roughness values were measured perpendicular to the horizontal bonding neck, whereas Flat values were measured perpendicular to the longitudinal bonding neck.

The experimental results demonstrate that build orientation significantly affects the formation of surface roughness in metal MEX. As summarized in Table 5 and Figure 10 and Figure 11 the average Rz values obtained for the Upright, Edge, and Flat orientations were 54.47 µm, 54.33 µm, and 27.37 µm, respectively. The observed roughness variation arises from the coupled interaction between deposition geometry and transient thermal behavior. Changes in build orientation alter the exposed surface area available for convective heat exchange, leading to different transient cooling histories during deposition. Faster heat dissipation shortens the effective coalescence period, thereby limiting bonding-neck growth before solidification and producing deeper interfacial valleys between adjacent filaments. In contrast, slower cooling prolongs the coalescence period, promotes neck growth, and progressively reduces the valley depth before sintering. Consequently, the measured roughness is consistent with the physical mechanism predicted by the proposed analytical framework, linking build orientation, transient heat transfer, bonding-neck evolution, and the final surface morphology.

Figure 10
Experimental and theoretical mean surface roughness values.
Figure 11
Distribution of surface roughness Rz.

This interpretation is supported by the experimental observations for the three build orientations discussed below. The Upright and Edge configurations exhibited nearly identical mean roughness values; however, their roughness dispersions differed markedly. The Upright orientation showed a standard deviation of 9.39 µm, whereas the Edge configuration exhibited a lower value of 3.17 µm, corresponding to an increase of approximately 196% in roughness variability, indicating stronger thermal instability during deposition in the Upright configuration.

The observed differences are closely associated with orientation-dependent transient heat transfer. In the Upright orientation, the larger exposed surface area and longer thermal path promote stronger convective heat dissipation, resulting in faster filament cooling and a shorter viscoelastic coalescence window. Under these conditions, the bonding neck between adjacent filaments cannot fully develop before solidification, leading to deeper interfacial valleys and increased surface roughness. Moreover, non-uniform heat extraction along the build height generates heterogeneous cooling conditions, which further amplifies fluctuations in bonding-neck evolution and contributes to the larger roughness dispersion observed experimentally.

By contrast, the Flat orientation provides more stable thermal conditions because the shorter thermal path and smaller exposed surface area reduce convective heat loss and prolong thermal retention within the deposited filament. This allows inter-filament coalescence to continue for a longer duration before solidification, promoting more extensive bonding-neck growth and gradual reduction of interfacial valley depth. In addition, the longitudinal bonding configuration in the Flat orientation provides a more continuous contact interface, resulting in a smoother surface profile and substantially lower roughness values.

The Edge orientation exhibited an intermediate thermal behavior between the Upright and Flat configurations. Although its average roughness remained close to that of the Upright orientation, the lower build height reduced thermal gradients and minimized local fluctuations in convective cooling. Consequently, the Edge samples exhibited more stable bonding-neck evolution and significantly lower roughness variability.

4.3. Prediction accuracy and roughness fluctuation analysis

Figure 12 shows that the analytical predictions remained close to the experimental measurements for all build orientations. The predicted roughness values for the Upright, Edge, and Flat configurations were 53.0 µm, 53.0 µm, and 26.6 µm, respectively, whereas the corresponding experimental averages reached 54.47 µm, 54.33 µm, and 27.37 µm. The resulting deviations were limited to 2.70%, 2.43%, and 2.80%, indicating that the proposed formulation reproduces the overall roughness level with good accuracy despite the simplified assumptions adopted in the thermal and rheological treatment.

Figure 12
Model vs. measurements.

The individual measurements exhibited noticeable scatter around the predicted values, particularly in the Upright orientation. In this case, the roughness ranged from 40.96 µm to 66.32 µm, corresponding to a fluctuation amplitude of approximately 25.4 µm. By comparison, the Edge specimens showed a considerably narrower interval, from 48.46 µm to 58.42 µm, with a fluctuation amplitude of about 10 µm. The Flat specimens exhibited intermediate dispersion, although the absolute roughness level remained substantially lower than that of the Upright and Edge configurations. The proposed model captures the dominant roughness formation mechanism, whereas the remaining deviations originate primarily from local variations in the deposition environment.

These fluctuations are likely associated with local variations in convective cooling during deposition. Since the model employs a nominal value of h1, it cannot fully reproduce transient airflow disturbances or spatial variations in heat dissipation occurring during layer deposition. Local increases in cooling intensity accelerate temperature decay and shorten the available coalescence period before solidification. As a result, neck growth becomes less extensive than predicted, leading to locally higher roughness values.

The analytical formulation assumes an effective viscosity representative of the overall deposition process, whereas the actual viscosity evolves continuously with local temperature. In regions where heat dissipation is more pronounced, the viscosity increases more rapidly, restricting viscous flow at the filament interface and slowing the coalescence process. Under these conditions, the interfacial valleys are not completely filled before solidification, producing localized increases in Rz.

Compared with our previous geometrical model [30], which estimates the final surface roughness primarily from the deposited filament geometry, layer height, and build orientation, the present framework incorporates the dominant physical mechanisms governing roughness evolution during metal MEX, including transient cooling, bonding-neck evolution, and sintering-induced shrinkage. As a result, the proposed model provides substantially improved predictive accuracy for the investigated Inconel 625 system while maintaining a clear physical interpretation of the roughness evolution process.

These results indicate that the proposed framework provides a physically consistent description of roughness evolution for the investigated material system and processing conditions. Because the formulation is expressed in terms of material and process parameters rather than material-specific empirical constants, it may be applicable to other metal MEX systems provided that the corresponding input properties are available. Nevertheless, its predictive accuracy under different filament compositions, printing parameters, and sintering conditions should be verified through additional experimental validation.

5. CONCLUSION

This study developed and validated a physics-based framework for predicting surface roughness in metal MEX using Inconel 625–polymer composite filaments. The model combines the geometrical representation of deposited filaments with the kinetics of bonding-neck evolution governed by surface-tension-driven viscous flow within a finite thermal window. Unlike conventional approaches, the formulation explicitly incorporates sintering-induced shrinkage, thereby enabling a direct transition from the green-state morphology to the final surface profile of the sintered part.

Based on a dataset comprising three build orientations (Upright, Edge, Flat) with nine measurement locations per orientation, the model reproduces the correct order of magnitude of surface roughness: Upright yields 54.47 µm versus a prediction of 53 µm (+2.77% deviation); Edge yields 54.33 µm versus 53 µm (+2.43%), and Flat yields 27.37 µm versus 26.60 µm (+2.88%). All experimental measurements fell within ±10 µm of the predicted values, indicating that the combined set of material, thermal, and geometric parameters successfully captured the roughness formation mechanisms associated with both bonding neck types.

From a physical perspective, surface roughness increases when the viscoelastic time tc is reduced due to faster heat dissipation, or when the effective viscosity η increases, limiting filament coalescence. Although the Upright and Edge orientations exhibit similar mean roughness, the Upright orientation shows greater variability, attributed to stronger thermal gradients along the build height. In contrast, the Flat orientation achieves lower roughness due to more stable thermal conditions and enhanced bonding neck growth prior to solidification

The proposed roughness model is simple yet effective, achieving an average prediction error of approximately 3% for the investigated material system and processing conditions. Although further validation is required for broader material systems and processing conditions, the proposed framework provides a practical pre-process prediction tool for metal material extrusion.

6. ACKNOWLEDGMENTS

This research is funded by University of Transport and Communications (UTC) under grant number T2025-CK-002TĐ.

7. DATA AVAILABILITY

The data that support the findings of this study are available from the corresponding author upon reasonable request.

8. BIBLIOGRAPHY

  • [1] ALTIPARMAK, S.C., YARDLEY, V.A., SHI, Z., et al, “Extrusion-based additive manufacturing technologies: State of the art and future perspectives.”, Journal of Manufacturing Processes, v. 83, pp. 607–636, 2022. doi: https://doi.org/10.1016/j.jmapro.2022.09.032.
    » https://doi.org/10.1016/j.jmapro.2022.09.032
  • [2] COSTA, J.M., SEQUEIROS, E.W., VIEIRA, M.F., “Fused filament fabrication for metallic materials: a brief review”, Materials (Basel), v. 16, n. 24, pp. 7505, 2023. doi: https://doi.org/10.3390/ma16247505. PubMed PMID: 38138650.
    » https://doi.org/10.3390/ma16247505
  • [3] CAO, D.L., NGUYEN, V.C., THI, V.N.T., “Microstructural and mechanical properties of 17-4PH stainless steel fabricated via material extrusion 3D printing”, Teknomekanik, v. 8, n. 1, pp. 67–78, 2025. doi: https://doi.org/10.24036/teknomekanik.v8i1.34872.
    » https://doi.org/10.24036/teknomekanik.v8i1.34872
  • [4] JACOB, J., PEJAK SIMUNEC, D., KANDJANI, A.E.Z., et al, “A review of fused filament fabrication of metal parts (Metal FFF): current developments and future challenges”, Technologies, v. 12, n. 12, pp. 267, 2024. doi: https://doi.org/10.3390/technologies12120267.
    » https://doi.org/10.3390/technologies12120267
  • [5] MUSA, N.H., MOHD YUSUF, S., ABU MANSOR, M., et al, “Material extrusion (MEX)-based additive manufacturing of metallic materials: review of current trends, challenges, and opportunities”, International Journal of Advanced Manufacturing Technology, v. 141, n. 12, pp. 5903–5929, 2025. doi: https://doi.org/10.1007/s00170-025-16832-w.
    » https://doi.org/10.1007/s00170-025-16832-w
  • [6] THOMPSON, Y., GONZALEZ-GUTIERREZ, J., KUKLA, C., et al, “Fused filament fabrication, debinding and sintering as a low-cost additive manufacturing method of 316L stainless steel”, Additive Manufacturing, v. 30, pp. 100861, 2019. doi: https://doi.org/10.1016/j.addma.2019.100861.
    » https://doi.org/10.1016/j.addma.2019.100861
  • [7] WAGNER, M.A., HADIAN, A., SEBASTIAN, T., et al, “Fused filament fabrication of stainless steel structures - from binder development to sintered properties”, Additive Manufacturing, v. 49, pp. 102472, 2022. https://doi.org/10.1016/j.addma.2021.102472.
  • [8] BANKAPALLI, N.K., GUPTA, V., SAXENA, P., et al, “Filament fabrication and subsequent additive manufacturing, debinding, and sintering for extrusion-based metal additive manufacturing and their applications: A review”, Composites. Part B, Engineering, v. 264, pp. 110915, 2023. doi: https://doi.org/10.1016/j.compositesb.2023.110915.
    » https://doi.org/10.1016/j.compositesb.2023.110915
  • [9] WAGNER, M.A., ENGEL, J., HADIAN, A., et al, “Filament extrusion-based additive manufacturing of 316L stainless steel: Effects of sintering conditions on the microstructure and mechanical properties.”, Additive Manufacturing, v. 59, pp. 103147, Nov. 2022. doi: https://doi.org/10.1016/j.addma.2022.103147.
    » https://doi.org/10.1016/j.addma.2022.103147
  • [10] BOSCHETTO, A., BOTTINI, L., “Roughness prediction in coupled operations of fused deposition modeling and barrel finishing”, Journal of Materials Processing Technology, v. 219, pp. 181–192, 2015. doi: https://doi.org/10.1016/j.jmatprotec.2014.12.021.
    » https://doi.org/10.1016/j.jmatprotec.2014.12.021
  • [11] LALEHPOUR, A., BARARI, A., “A more accurate analytical formulation of surface roughness in layer-based additive manufacturing to enhance the product’s precision”, International Journal of Advanced Manufacturing Technology, v. 96, n. 9–12, pp. 3793–3804, 2018. doi: https://doi.org/10.1007/s00170-017-1448-x.
    » https://doi.org/10.1007/s00170-017-1448-x
  • [12] JIANG, S., HU, K., ZHAN, Y., et al, “Theoretical and experimental investigation on the 3D surface roughness of material extrusion additive manufacturing products”, Polymers, v. 14, n. 2, pp. 293, 2022. https://doi.org/10.3390/polym14020293. PubMed PMID: 35054698.
  • [13] LEPOIVRE, A., BOYARD, N., LEVY, A., et al, “Methodology to assess interlayer quality in the material extrusion process: A temperature and adhesion prediction on a high performance polymer.”, Additive Manufacturing, v. 60, pp. 103167, 2022. doi: https://doi.org/10.1016/j.addma.2022.103167.
    » https://doi.org/10.1016/j.addma.2022.103167
  • [14] COOGAN, T.J., KAZMER, D.O., “Prediction of interlayer strength in material extrusion additive manufacturing”, Additive Manufacturing, v. 35, pp. 101368, 2020. doi: https://doi.org/10.1016/j.addma.2020.101368.
    » https://doi.org/10.1016/j.addma.2020.101368
  • [15] COOGAN, T.J., KAZMER, D.O., “Modeling of interlayer contact and contact pressure during fused filament fabrication”, Journal of Rheology (New York, N.Y.), v. 63, n. 4, pp. 655–672, Jul. 2019. doi: https://doi.org/10.1122/1.5093033.
    » https://doi.org/10.1122/1.5093033
  • [16] FRENKEL, J., ESHELBY, J., “Viscous flow of crystalline bodies under the action of surface tension, discussion of seminar on the kinetics of sintering”, J. Phys. Metallurgical Transactions, v. 9, pp. 385, 1945.
  • [17] LEPOIVRE, A., BOYARD, N., LEVY, A., et al, “Heat transfer and adhesion study for the FFF additive manufacturing process”, Procedia Manufacturing, v. 47, pp. 948–955, 2020. doi: https://doi.org/10.1016/j.promfg.2020.04.291.
    » https://doi.org/10.1016/j.promfg.2020.04.291
  • [18] DEFAUCHY, D., “Simulation du procédé de fabrication directe de pièces thermoplastiques par fusion laser de poudre”, D.Sc. Thesis, Paris, Institute of Technology, ENSAM, 2013.
  • [19] BAKRANI BALANI, S., ARTHUR, C., FRANCE, C., et al, “Influence of parameters controlling the extrusion step in fused filament fabrication (FFF) process applied to polymers using numerical simulation”, In: AIP Conference Proceedings, v. 1960, 2018.
  • [20] BUJ-CORRAL, I., DOMÍNGUEZ-FERNÁNDEZ, A., DURÁN-LLUCIÀ, R., “Influence of print orientation on surface roughness in Fused Deposition Modeling (FDM) processes”, Materials (Basel), v. 12, n. 23, pp. 3834, 2019. doi: https://doi.org/10.3390/ma12233834. PubMed PMID: 31766409.
    » https://doi.org/10.3390/ma12233834
  • [21] ABAS, M., AWADH, M.A., HABIB, T., et al, “Analyzing surface roughness variations in material extrusion additive manufacturing of nylon carbon fiber composites”, Polymers, v. 15, n. 17, pp. 3633, 2023. doi: https://doi.org/10.3390/polym15173633. PubMed PMID: 37688259.
    » https://doi.org/10.3390/polym15173633
  • [22] JIN, Y., LI, H., HE, Y., et al, “Quantitative analysis of surface profile in fused deposition modelling”, Additive Manufacturing, v. 8, pp. 142–148, 2015. doi: https://doi.org/10.1016/j.addma.2015.10.001.
    » https://doi.org/10.1016/j.addma.2015.10.001
  • [23] VANAEI, H.R., DELIGANT, M., SHIRINBAYAN, M., et al, “A comparative in-process monitoring of temperature profile in fused filament fabrication”, Polymer Engineering and Science, v. 6, n. 1, pp. 1–9, 2020. doi: https://doi.org/10.1002/pen.25555.
    » https://doi.org/10.1002/pen.25555
  • [24] VANAEI, H.R., SHIRINBAYAN, M., DELIGANT, M., et al, “In-process monitoring of temperature evolution during fused filament fabrication: a journey from numerical to experimental approaches”, Thermo, v. 1, n. 3, pp. 332–360, 2021. doi: https://doi.org/10.3390/thermo1030021.
    » https://doi.org/10.3390/thermo1030021
  • [25] ASAMI, K., KUEHNE, M., RÖVER, T., et al, “Application of machine learning in predicting quality parameters in Metal Material Extrusion (MEX/M).”, Metals, v. 15, n. 5, pp. 505, 2025. doi: https://doi.org/10.3390/met15050505.
    » https://doi.org/10.3390/met15050505
  • [26] TRAN, T.V.N., LONG, D.C., VAN, C.N., “The influence of printing materials on shrinkage characterization in metal 3d printing using material extrusion technology”, Engineering, Technology & Applied Science Research, v. 14, n. 4, pp. 15356–15360, Aug. 2024. doi: https://doi.org/10.48084/etasr.7758.
    » https://doi.org/10.48084/etasr.7758
  • [27] BETTS, J.L., SAMPSON, B.J., LINDSEY, K., et al, “Reduction of process induced porosity for ultrafuse 316L through parameter optimization of creality ender 3 V2 and makerbot method X”, Crystals, v. 14, n. 3, pp. 285, 2024. doi: https://doi.org/10.3390/cryst14030285.
    » https://doi.org/10.3390/cryst14030285
  • [28] EICKHOFF, R., ANTUSCH, S., BAUMGÄRTNER, S., et al, “Feedstock development for material extrusion-based printing of Ti6Al4V parts”, Materials (Basel), v. 15, n. 18, pp. 6442, 2022. doi: https://doi.org/10.3390/ma15186442. PubMed PMID: 36143753.
    » https://doi.org/10.3390/ma15186442
  • [29] SUWANPREECHA, C., MANONUKUL, A., “A review on material extrusion additive manufacturing of metal and how it compares with metal injection moulding”, Metals, v. 12, n. 3, pp. 429, 2022. doi: https://doi.org/10.3390/met12030429.
    » https://doi.org/10.3390/met12030429
  • [30] VAN, C.N., HOANG, A.L., LONG, C.D., et al, “Surface roughness in metal material extrusion 3D printing: the influence of printing orientation and the development of a predictive model”, Engineering, Technology & Applied Science Research, v. 13, n. 5, pp. 11672–11676, Oct. 2023. https://doi.org/10.48084/etasr.6162.
  • [31] TOFAIL, S.A.M., KOUMOULOS, E.P., BANDYOPADHYAY, A., et al, “Additive manufacturing: scientific and technological challenges, market uptake and opportunities”, Materials Today, v. 21, n. 1, pp. 22–37, 2018. doi: https://doi.org/10.1016/j.mattod.2017.07.001.
    » https://doi.org/10.1016/j.mattod.2017.07.001
  • [32] HOFFMANN, M., ELWANY, A., “Material extrusion additive manufacturing of AISI 316L pastes.”, Journal of Manufacturing Processes, v. 108, pp. 238–251, 2023. doi: https://doi.org/10.1016/j.jmapro.2023.10.078.
    » https://doi.org/10.1016/j.jmapro.2023.10.078
  • [33] DANG, L.C., NGUYEN, C.V., LE, A.H., et al, “A study on the influence of printing orientation in metal printing using material extrusion technology on the mechanical properties of 17–4 stainless steel products”, Journal of Machine Engineering, v. 23, n. 4, pp. 89–100, 2023. doi: https://doi.org/10.36897/jme/170509.
    » https://doi.org/10.36897/jme/170509
  • [34] YANG, Y., LI, B., CHE, L., et al, “Calculation model and influence factors of thermal conductivity of composite cement-based materials for geothermal well”, Geothermal Energy, v. 12, n. 1, pp. 3, 2024. doi: https://doi.org/10.1186/s40517-024-00282-w.
    » https://doi.org/10.1186/s40517-024-00282-w
  • [35] LUSICINI, D., CRACHI, M., SESANA, R., et al, “Experimental analysis of thermomechanical properties of innovative heat treated metal matrix composites processed by additive manufacturing for space rocket applications”, Journal of Materials Engineering and Performance, v. 34, n. 17, pp. 19824–19839, 2025. doi: https://doi.org/10.1007/s11665-025-11165-x.
    » https://doi.org/10.1007/s11665-025-11165-x
  • [36] KISWANTO, G., KHOLIL, A., ISTIYANTO, J., “Effect of infill pattern on impact toughness, microstructure, and surface roughness of inconel 625 built via filament-based material extrusion additive manufacturing”, J. Manuf. Mater. Process., v. 7, n. 3, pp. 114, 2023. doi: https://doi.org/10.3390/jmmp7030114.
    » https://doi.org/10.3390/jmmp7030114

Corresponding Author:

Cuong Nguyen Van, duynh@vlute.edu.vn, nguyencuong@utc.edu.vn, anhlh@vlute.edu.vn

Publication Dates

  • Publication in this collection
    12 Oct 2026
  • Date of issue
    2026

History

  • Received
    13 May 2026
  • Accepted
    13 Aug 2026
location_on
Laboratório de Hidrogênio, Coppe - Universidade Federal do Rio de Janeiro, em cooperação com a Associação Brasileira do Hidrogênio, ABH2 Av. Moniz Aragão, 207, 21941-594, Rio de Janeiro, RJ, Brasil, Tel: +55 (21) 3938-8791 - Rio de Janeiro - RJ - Brazil
E-mail: revmateria@gmail.com
rss_feed Acompanhe os números deste periódico no seu leitor de RSS
Ir para o topo