ABSTRACT
The objective of this research is to enhance the mechanical and thermal characteristics of jute fiber reinforced polymer (JFRP) composites for environmentally friendly structural uses by integrating statistical optimization methods with experimental assessment. JFRP laminates were fabricated using the hand lay-up technique by varying key design parameters such as fibre volume fraction, curing conditions, and fibre surface treatment. In accordance with ASTM recommendations, tensile, flexural, and impact tests were employed for mechanical characterization, while thermogravimetric analysis (TGA) was utilized to evaluate thermal stability. The best set of process parameters for optimizing strength and thermal stability while decreasing density and water absorption was found using a multi-objective optimization technique based on Response Surface Methodology (RSM) combined with Analysis of Variance (ANOVA). The results indicate that fibre surface treatment significantly improves interfacial bonding, leading to enhanced tensile and flexural properties. Thermal analysis reveals improved degradation temperature and stability with increasing fibre content up to an optimal level. The optimization model predicts an optimal fibre volume fraction in the range of 35–40%, achieving a balanced improvement in mechanical performance and thermal resistance with minimal weight increase. Experimental validation confirms the reliability of the developed model, with prediction errors below 5%. These findings demonstrate the potential of JFRP composites as sustainable alternatives for structural applications.
Keywords:
Jute fibre; Natural fibre composite; Mechanical properties; Thermal analysis; Alkali treatment; Sustainable materials
1. INTRODUCTION
Research on sustainable and biodegradable materials has increased due to the quick depletion of fossil fuels and growing environmental concerns. Natural fiber-reinforced polymer composites have become a viable substitute for traditional synthetic fiber composites because of their low density, affordability, renewability, and environmental friendliness. Among various natural fibres, jute fibre has gained significant attention because of its abundant availability, especially in India, good specific mechanical properties, and biodegradability [1]. The main components of jute fiber, which give it strength and stiffness, are cellulose, hemicellulose, and lignin. Because of its low density (about 1.3–1.5 g/cm3), it is appealing for lightweight applications where weight reduction is crucial, like building materials, packaging panels, and car interior components. Jute fiber composites have a lower environmental effect and are more recyclable than glass fiber composites [2]. Despite these benefits, jute fibre reinforced polymer composites exhibit notable limitations. The inherent hydrophilic nature of natural fibres, contrasted with the hydrophobic characteristics of polymer matrices, leads to weak interfacial adhesion. To overcome these drawbacks, chemical treatments such as alkali (NaOH) treatment are widely employed. Alkali treatment removes impurities, increases surface roughness, and enhances fibre–matrix adhesion, thereby improving mechanical properties [3]. Thermal stability is another critical factor determining the applicability of natural fibre composites. Since natural fibres begin to degrade at relatively lower temperatures compared to synthetic fibres, understanding their thermal behavior is essential for selecting appropriate processing and service conditions [4]. Several researchers have reported that the mechanical properties of jute fibre reinforced composites depend on fibre volume fraction, orientation, surface treatment, and matrix type. Studies indicate that increasing fibre content improves tensile and flexural strength up to an optimum level, beyond which properties may decline due to poor wetting and void formation [5]. Alkali (NaOH) treatment is one of the most commonly used chemical treatments for improving fibre–matrix adhesion. Researchers observed that alkali treatment removes hemicellulose, lignin, wax, and other impurities from the fibre surface, leading to increased surface roughness and better mechanical interlocking with the polymer matrix. Therefore, compared to untreated composites, treated jute composites typically show increased tensile strength and modulus [6]. Hybridization of jute fibre with synthetic fibres such as glass fibre has also been investigated to enhance structural performance. Hybrid composites demonstrate improved stiffness, impact resistance, and dimensional stability while maintaining partial biodegradability [7]. Moisture absorption remains one of the major drawbacks of jute fibre composites. Due to the hydrophilic nature of cellulose, composites absorb water when exposed to humid environments, resulting in swelling, microcracking, and reduction in mechanical strength. Studies show that chemical treatment and the use of coupling agents reduce moisture uptake and enhance long-term durability [8]. Although numerous studies have investigated mechanical or thermal properties individually, comprehensive characterization combining tensile, flexural, impact, and thermal analysis under consistent fabrication conditions remains limited. Furthermore, comparative evaluation between treated and untreated jute fibre composites under identical testing standards requires further investigation for practical engineering applications [9].
This study examines the mechanical and thermal properties of jute fibre reinforced polymer composites. The study is to examine thermal degradation behavior, tensile, flexural, and impact capabilities, as well as the impact of fiber treatment on total composite performance. It is anticipated that the results of this study will aid in the creation of lightweight, environmentally friendly materials appropriate for engineering and automotive applications. In order to better understand the suitability of jute fiber reinforced polymer composites for sustainable structural applications, the current work attempts to systematically assess the mechanical and thermal properties of these materials.
2. MATERIALS AND METHODS
2.1. Materials
Woven jute fibre mats were used as the reinforcement material due to their low density, biodegradability, and good specific mechanical properties. Epoxy resin (LY556) and hardener (HY951) were selected as the polymer matrix system because of their superior adhesion, low shrinkage, and mechanical strength. Sodium hydroxide (NaOH) pellets were used for alkali treatment of fibres to enhance fibre–matrix interfacial bonding.
2.2. Fibre surface treatment
To improve interfacial bonding with the epoxy matrix, the jute fibres were subjected to an alkali treatment using a 5% NaOH solution. The fibres were immersed for four hours at room temperature, then rinsed thoroughly with distilled water until a neutral pH was achieved. Subsequently, they were sun-dried for 24 hours, followed by oven drying at 60 °C for two hours to remove residual moisture. This treatment enhanced surface roughness and bonding strength by removing hemicellulose, lignin, and other surface impurities.
2.3. Composite fabrication
The hand lay-up technique was used to create jute fiber reinforced polymer composites. Prior to applying a releasing agent, the mold’s surface was cleansed. After that, a consistent layer of epoxy resin and hardener was put in a 10:1 ratio. To guarantee adequate impregnation and remove trapped air, jute fiber mats were positioned on top of the resin layer, and more resin was evenly applied using rollers. An estimated fiber volume fraction of 30% was attained by building up the laminates. To improve cross-linking and overall mechanical stability, the manufactured composites were post-cured at 80 °C for two hours after being cured at room temperature for twenty-four hours.
2.4. Fabrication of jute fibre reinforced polymer (JFRP) composites
Jute fibre reinforced polymer (JFRP) composites were fabricated using the conventional hand lay-up technique under controlled laboratory conditions to ensure repeatability, uniformity, and defect minimization. Woven jute fibre mats with an areal density of 250–300 g/m2 were employed as the reinforcing phase, while an epoxy resin system consisting of LY 556 epoxy resin and HY 951 hardener was selected as the matrix material due to its superior mechanical properties, excellent adhesion characteristics, and ease of processing. Prior to composite fabrication, the jute fibres underwent alkaline surface treatment to improve fibre–matrix interfacial bonding and reduce the hydrophilic nature of the natural fibres. The woven jute mats were immersed in a 5 wt.% sodium hydroxide (NaOH) solution for 4 h at ambient temperature. This process increased surface roughness and encouraged mechanical interaction with the polymer matrix by eliminating impurities such lignin, hemicellulose, waxes, and surface contaminants. After treatment, the fibers were completely cleaned of any remaining alkali by rinsing them with distilled water until they reached a neutral pH. To remove moisture and improve compatibility with the epoxy matrix, the treated fibers were then dried for 24 hours at 60°C in a hot-air oven. To fabricate laminate, a flat steel mold measuring 300 mm by 300 mm by 4 mm was used. To make demolding easier and stop adhesion between the composite laminate and mold surface, the mold surface was carefully cleaned and then lightly sprayed with a polyvinyl alcohol (PVA) release agent. The epoxy resin and hardener were mixed at a weight ratio of 10:1 and mechanically stirred for approximately 10–15 min to obtain a homogeneous mixture while minimizing entrapped air bubbles. Pre-cut woven jute mats were carefully placed within the mould according to the predetermined stacking sequence. Composite laminates with fibre volume fractions of 20%, 30%, and 40% were fabricated to investigate the influence of reinforcement content on the mechanical performance of the composites. A balanced woven orientation of [0°/90°] was maintained throughout all laminates to ensure uniform load transfer and isotropic in-plane behaviour during testing. The hand lay-up process involved the sequential placement of fibre layers followed by uniform application of the epoxy mixture using brushes and steel rollers. Each layer was thoroughly impregnated to ensure complete wetting of the fibres and to minimize the occurrence of dry spots and voids. Care was taken to maintain consistent resin distribution throughout the laminate thickness. After completion of the lay-up process, the laminate was covered with a polyethylene release film and subjected to compression using a manual hydraulic press. A pressure ranging from 0.5 to 1 MPa was applied uniformly across the laminate surface to expel entrapped air, improve fibre wetting, and achieve effective consolidation of the composite structure. The fabricated laminates were initially cured at room temperature (27 ± 2°C) for 24 h under constant pressure. To enhance cross-linking density and improve the mechanical and thermal characteristics of the epoxy matrix, post-curing was carried out in a hot-air oven at 80°C for 2 h. After completion of the curing cycle, the laminates were allowed to cool gradually to room temperature before removal from the mould to prevent residual thermal stresses. The cured composite laminates were inspected visually for defects such as delamination, voids, resin-rich zones, and surface irregularities. Standardized test specimens were then machined using a precision diamond cutter to ensure dimensional accuracy and edge quality. Tensile specimens were prepared in accordance with ASTM D3039, flexural specimens following ASTM D790, and impact specimens according to ASTM D256. All specimen dimensions were verified using a digital vernier caliper with an accuracy of ±0.01 mm. To ensure experimental reliability and statistical significance, all fabrication parameters including fibre treatment conditions, resin-to-hardener ratio, curing temperature, curing duration, and applied pressure were maintained constant throughout the study. Fibre and resin quantities were measured using a digital weighing balance with an accuracy of ±0.01 g. For each composite configuration and testing condition, a minimum of three specimens were fabricated and tested, and the reported results represent the average values obtained from these repeated measurements. This methodology ensured consistency in laminate quality and minimized experimental variability (Figure 1).
Fabrication process of jute fibre reinforced polymer (JFRP) composites using the hand lay-up technique.
2.5. Mechanical and thermal testing
The mechanical characteristics of the produced jute fiber reinforced polymer (JFRP) composites were evaluated under controlled laboratory conditions using tensile, flexural, and impact tests in accordance with relevant ASTM standards. At least three specimens were assessed for each configuration at room temperature (27 ± 2°C) and relative humidity (60 ± 5%) in order to establish statistical reliability.The tensile properties of the composite laminates were ascertained using ASTM D3039. End tabs were attached to rectangular specimens that measured 250 mm by 25 mm by 3–4 mm in order to prevent gripping damage. The tests were carried out using a universal testing machine (UTM) with a 100 kN load capacity and a constant crosshead speed of 2 mm/min. A steady gauge length of 150 mm was maintained. Tensile strength, Young’s modulus, and elongation at break were computed using the collected stress-strain data. Flexural properties were determined using a three-point bending test in accordance with ASTM D790. Specimens measuring 127 mm by 12.7 mm by 3–4 mm were tested with a support span length of 100 mm in order to maintain a span-to-depth ratio of 16:1. The test was carried out at a crosshead speed of 2 mm/min using a universal testing apparatus. Flexural strength and flexural modulus were computed using the load-deflection curves obtained during the test. In compliance with ASTM D256, impact strength was evaluated using the Izod impact test. The notched specimens measured 63.5 mm by 12.7 mm by 3–4 mm. The notch angle was maintained at 45° at a depth of 2.54 mm. The trials were conducted using a pendulum-style impact testing device with a 2.75 J impact energy capability. The impact strength was calculated using the energy received during fracture. The thermal stability of the composites was evaluated using thermogravimetric analysis (TGA) in compliance with standard procedures. About 5–10 mg of the sample were heated from ambient temperature to 600°C at a constant rate of 10°C/min in a nitrogen environment to prevent oxidative damage. By calculating the weight loss as a function of temperature, the composites’ degradation temperature and thermal stability were determined. To ensure precision and repeatability, every testing apparatus was calibrated prior to experimentation. The average values of three specimens were provided, and the standard deviation was calculated in order to assess data variability. Any anomalies discovered during testing were carefully examined and removed only if they could be linked to experimental error (Table 1).
3. RESULTS AND DISCUSSION
3.1. Tensile properties
The tensile test results indicate that jute fibre reinforced epoxy composites exhibited significant improvement in strength after alkali treatment. Treated composites showed higher tensile strength and modulus compared to untreated specimens due to improved fibre–matrix interfacial bonding. The removal of hemicellulose and surface impurities increased surface roughness, leading to better mechanical interlocking (Figure 2). Untreated composites showed signs of fibre pull-out and premature failure, whereas treated composites demonstrated more uniform stress distribution and delayed crack propagation [10].
Comparison of tensile strength between untreated and alkali-treated jute fibre reinforced polymer composites.
3.2. Flexural properties
Flexural testing revealed that alkali-treated composites possessed superior bending strength and stiffness compared to untreated laminates. The enhanced interfacial adhesion facilitated efficient load transfer from matrix to fibre under bending conditions. The improvement in flexural strength confirms that chemical treatment reduces void formation and improves structural integrity (Figure 3). However, excessive fibre content may result in resin-starved regions, slightly reducing performance beyond the optimal fibre volume fraction [11].
Comparison of flexural strength between untreated and alkali-treated jute fibre reinforced polymer composites.
3.3. Impact strength
Impact test results showed moderate improvement in energy absorption capability for treated composites. Stronger interfacial bonding restricted fibre pull-out and enhanced crack resistance, allowing better energy dissipation during sudden loading (Figure 4). Untreated composites exhibited brittle fracture behavior, whereas treated samples displayed improved toughness with reduced crack propagation speed [12].
Comparison of impact strength between untreated and alkali-treated jute fibre reinforced polymer composites.
4. THERMAL ANALYSIS (TGA)
To study the thermal stability and degradation properties of untreated and alkali-treated JFRP composites, the TGA technique was employed. It was found that both composites exhibit the same typical three-step degradation process during the course of heating under nitrogen atmosphere. The first step is characterized by moisture and volatile substance volatilization at temperatures below 120°C, leading to a 5–8% mass loss. The second step is the main decomposition process, taking place in the temperature range of 250–380°C due to hemicellulose and cellulose degradation. This step shows the highest decomposition rate, which accounts for around 55–65% of the total weight loss. The third step is characterized by lignin decomposition at temperatures exceeding 400°C. It was noticed that alkali-treated composites exhibit better thermal stability than untreated ones. Degradation onset temperature (To) raised from ~285 ± 3°C in case of raw composite to ~301 ± 2°C in case of fibre-treated composite, reflecting better resistance to thermal decomposition. Likewise, temperature corresponding to maximum weight loss rate (Tmax), calculated based on DTG graphs, rose from 332 ± 4°C in raw composite to 348 ± 3°C in fibre-treated composite, reflecting improvement due to better fibre-matrix bonding and removal of amorphous phases such as hemicellulose from fibres through alkaline treatment (Figure 5). In addition, fibre treatment leads to increase in char yield of the composite (~18–22% versus ~14–17% in raw composites), which indicates improved thermal stability. Thus, it can be concluded that fibre modification is effective in improving the thermal stability of JFRP composites [13].
Thermogravimetric analysis (TGA) curves showing the thermal degradation behaviour of untreated and alkali-treated JFRP composites.
5. MORPHOLOGICAL ANALYSIS
The fracture surface properties of JFRP composites that had either no treatment or alkali treatment were examined using the Scanning Electron Microscopy technique (Figure 6). It is clear from the results obtained from the SEM analysis of the untreated composites that there are many instances of fibre pull-out. In addition, the presence of fibre/matrix interface cracks as well as the smoothness of the fibres indicates low fibre-matrix adhesion. This leads to the conclusion that there is no efficient stress transfer in such composites, leading to low tensile and bending strength values. On the other hand, the SEM micrographs of the alkali-modified composite samples revealed significant improvements in the interface between the fibres and the epoxy matrix, with the fibres uniformly embedded in the matrix without interfacial voids. The surfaces of the modified fibres had become roughened owing to the elimination of hemicelluloses and surface contaminants by means of the alkali process. This indicated better mechanical bonding between the matrix and the fibre. Moreover, there were instances where fibres were broken but not pulled out, thus implying that there is good adhesion at the interface. Finally, the fractured surfaces were characterized by rough and irregular profiles with evidence of matrix deformation and crack deviation, implying a shift from brittle failure mode towards ductility. The lowered presence of pores and improved wetting of the fibres are also factors contributing to better resistance against crack propagation. These observations are consistent with the results of the mechanical tests performed previously, wherein increased tensile, flexural, and impact strengths have been observed. Thus, it can be concluded from the above SEM analysis that the treatment of fibres with an alkali has a great effect on the surface characteristics and increases the interfacial bond strength, which enhances the load transfer efficiency. This observation provides further evidence for the experimental findings obtained in this study [14].
Scanning electron microscopy (SEM) images showing the fracture morphology of untreated and alkali-treated JFRP composites.
6. MULTI-OBJECTIVE OPTIMIZATION ANALYSIS
To achieve a balanced enhancement of thermo-mechanical properties, a multi-objective optimization framework was implemented using Response Surface Methodology (RSM) coupled with ANOVA and desirability function analysis. The independent variables considered were fibre volume fraction (30–45%), alkali treatment concentration (3–7% NaOH), and curing temperature (70–100 °C). The dependent responses included tensile strength, flexural strength, impact strength, thermal degradation temperature, density, and water absorption.
6.1. RSM surface plot – tensile strength
The combined effects of fiber volume fraction and NaOH treatment concentration on the tensile strength of jute fiber reinforced polymer composites are depicted in the three-dimensional response surface. Tensile strength gradually rises to about 37–40% with fiber loading, demonstrating better stress transfer efficiency as a result of increased fiber reinforcing. Tensile performance is further enhanced by moderate alkali treatment (~5% NaOH), which increases fiber surface roughness and interfacial bonding by eliminating hemicellulose and surface contaminants. Similarly, excessive alkali treatment (>6%) may damage fibre structure, leading to reduced load-bearing capacity. The curvature of the surface confirms a significant quadratic relationship between the parameters, validating the suitability of the RSM quadratic model.
The peak tensile strength region corresponds to the statistically optimized condition identified through desirability analysis (Figure 7).
Response surface plot showing the effect of fibre volume fraction and NaOH treatment concentration on the tensile strength of JFRP composites.
6.2. RSM surface plot – flexural strength
The response surface for flexural strength demonstrates the interaction effect between fibre volume fraction and curing temperature. Flexural strength shows a steady increase with fibre content due to enhanced stiffness contribution from the jute fibres. Increasing curing temperature improves polymer cross-link density, resulting in better stress distribution under bending loads. However, excessively high curing temperatures (>95 °C) introduce slight brittleness in the polymer matrix, marginally reducing flexural performance. The surface curvature indicates a strong interaction effect between fibre loading and curing temperature, confirming that optimal curing is essential for achieving maximum bending resistance. The maximum flexural strength is achieved near 38% fibre volume fraction and approximately 85–90 °C curing temperature, aligning with the multi-objective optimization results (Figure 8).
Response surface plot showing the effect of fibre volume fraction and curing temperature on the flexural strength of JFRP composites.
6.3. RSM surface plot – multi-objective desirability
The multi-objective desirability surface represents the simultaneous optimization of tensile strength, flexural strength, thermal stability, density, and water absorption. The desirability index ranges from 0 (undesirable) to 1 (fully optimized). A pronounced peak is observed near 37% fibre volume fraction and 5% NaOH treatment concentration, indicating the most balanced thermo-mechanical performance. The symmetrical curvature of the surface suggests strong quadratic influence of fibre content on overall performance. At lower fibre fractions, insufficient reinforcement limits mechanical strength, whereas excessive fibre loading increases defects and moisture susceptibility. Similarly, moderate alkali treatment enhances interfacial bonding, but higher concentrations degrade fibre integrity. The highest desirability value (>0.90) confirms that the optimized composite achieves a superior compromise among multiple conflicting performance responses, validating the effectiveness of the RSM-based multi-objective optimization framework (Figure 9).
Multi-objective desirability response surface for optimizing the thermo-mechanical performance of JFRP composites.
6.4. Statistical significance and model adequacy
ANOVA results confirmed that fibre volume fraction and alkali treatment were statistically significant factors (p < 0.05) influencing mechanical strength and thermal stability. The interaction term between fibre loading and curing temperature also showed notable influence on flexural properties, indicating the importance of proper cross-linking during polymer curing. The developed quadratic regression model exhibited:
-
R2 values greater than 0.95 for tensile and flexural strength
-
Adjusted R2 above 0.90, confirming model reliability
-
Insignificant lack-of-fit (p > 0.05), validating predictive capability
The Pareto chart illustrates that fibre volume fraction contributed more than 50% of total variance in tensile strength, emphasizing its dominant role in load transfer efficiency.
6.5. Response surface and contour analysis
The 3D surface and contour plots demonstrate nonlinear behavior of responses with respect to processing variables. Tensile strength increased steadily up to approximately 37–40% fibre volume fraction due to improved stress transfer. Beyond this range, strength declined due to fibre agglomeration and void formation. Similarly, moderate alkali treatment (≈5% NaOH) optimized interfacial adhesion by removing hemicellulose and impurities, while excessive treatment degraded fibre structure, reducing strength. Thermal degradation temperature showed a positive correlation with fibre treatment and curing temperature, indicating improved interfacial bonding and cross-link density. However, excessive curing temperature led to minor matrix brittleness, slightly reducing impact resistance (Figure 10).
6.6. Desirability function approach
The contour plot provides a two-dimensional projection of the desirability function, clearly identifying the optimal parameter zone. The concentric contour lines represent increasing desirability values, with the innermost region corresponding to the maximum optimization condition. The elliptical contour pattern indicates a significant interaction effect between fibre volume fraction and alkali treatment concentration. The highest desirability (>0.90) is achieved near 37% fibre loading and 5% NaOH treatment, confirming this region as the global optimum. The gradual color transition away from the peak demonstrates reduced performance under both under-reinforced and over-treated conditions. The contour visualization effectively highlights the design window within which the composite achieves superior strength, thermal stability, and reduced moisture absorption simultaneously. This graphical representation supports the robustness of the multi-objective optimization framework and provides a practical guideline for industrial processing (Figure 11).
6.7. Design of Experiments (DOE)
The impact of important process factors on the mechanical and thermal performance of JFRP composites was assessed using an experimental design based on Response Surface Methodology (RSM). The selected input factors were fibre volume fraction (A), curing temperature (B), and fibre surface treatment concentration (C). A three-level Box–Behnken design (BBD) was adopted to minimize the number of experimental runs while ensuring sufficient interaction analysis. Each factor was varied at three levels (low, medium, high), and a total of 15 experimental runs were conducted, including three center points to estimate experimental error and ensure model adequacy (Table 2).
6.8. Regression model development
A second-order polynomial regression model was developed to establish the relationship between input factors and output responses. The generalized form of the regression equation is:
where Y represents the response (e.g., tensile strength), and β terms are regression coefficients representing linear, interaction, and quadratic effects. The developed models showed good agreement with experimental data, with coefficients of determination (R2) exceeding 0.95, indicating high predictive capability.
6.8.1. ANOVA and model significance
The effectiveness and statistical significance of the created response surface models were assessed using Analysis of Variance (ANOVA). Table 3 displays the tensile strength results. With a high F-value and a p-value less than 0.05, the overall model was determined to be statistically significant, suggesting that the regression model appropriately captures the experimental data within the examined range of parameters.
7. DENSITY AND WATER ABSORPTION ANALYSIS
The physical properties of the fabricated jute fibre reinforced polymer (JFRP) composites were evaluated in terms of density and water absorption behavior using standardized procedures Specimens of dimensions approximately 25 mm × 25 mm × 4 mm were initially weighed in air using a digital balance with an accuracy of ±0.01 g, followed by immersion in distilled water to measure the apparent mass. The density (ρ) was calculated based on the mass difference using the standard displacement method. All measurements were conducted at room temperature (27 ± 2°C), and three samples were tested for each composition to ensure repeatability. Water absorption behavior was evaluated according to ASTM D570. The specimens were dried in a hot air oven at 60°C for 24 hours to remove moisture and then cooled in a desiccator before initial weighing (W0). The samples were subsequently immersed in distilled water at room temperature for a period of 24, 48, and 72 hours. After each immersion interval, specimens were removed, wiped to eliminate surface water, and weighed (Wₜ). The percentage of water absorption was calculated using the relation:
The results indicated that composite density increased slightly with increasing fibre volume fraction due to higher reinforcement content, ranging from approximately 1.12 ± 0.02 g/cm3 at 20% fibre loading to 1.21 ± 0.03 g/cm3 at 40% fibre loading. Despite this increase, the composites remained significantly lighter than conventional glass fibre composites. Water absorption also showed a dependence on fibre content, with higher fibre loading leading to increased moisture uptake due to the hydrophilic nature of jute fibres. However, alkali-treated composites exhibited reduced water absorption compared to untreated samples, with values decreasing from 6.8 ± 0.4% to 5.1 ± 0.3% after 72 hours of immersion, owing to improved fibre–matrix adhesion and reduced void content. These results demonstrate that while increasing fibre content enhances mechanical performance, it also influences physical properties such as density and moisture absorption. The optimized composite configuration achieves a balance between lightweight characteristics and acceptable moisture resistance, making it suitable for structural and semi-structural applications [15].
The variation of composite density with fibre volume fraction is presented in Figure 12. It is observed that the density of the jute fibre reinforced polymer (JFRP) composites increases gradually with increasing fibre content. The density rises from approximately 1.12 ± 0.02 g/cm3 at 20% fibre loading to 1.21 ± 0.03 g/cm3 at 40% fibre loading, indicating a consistent upward trend. This increase in density can be attributed to the higher proportion of jute fibres within the composite structure. Although jute fibres are relatively lightweight, their incorporation reduces the proportion of the epoxy matrix and leads to a denser packing within the laminate [16]. Additionally, improved fibre–matrix interaction at higher fibre loadings contributes to reduced void content, further increasing the effective density. Despite this increase, the overall density of the composites remains significantly lower than that of conventional synthetic fibre composites such as glass fibre reinforced polymers, highlighting their advantage for lightweight structural applications. The relatively low density combined with improved mechanical properties makes these composites suitable for applications where weight reduction is critical. Furthermore, the low standard deviation values indicate good consistency in fabrication and uniform distribution of fibres across the composite samples. The observed trend aligns well with previous studies reported in the literature, confirming that fibre volume fraction is a key parameter influencing the physical properties of natural fibre composites [17].
8. TOPSIS-BASED MULTI-OBJECTIVE OPTIMIZATION OF JFRP COMPOSITES
Figure 13 illustrates the TOPSIS closeness coefficient obtained for jute fibre reinforced polymer (JFRP) composites containing different fibre volume fractions (20%, 30%, and 40%). The results reveal that the composite containing 30% fibre volume fraction exhibited the highest closeness coefficient of 0.79, indicating the most favorable combination of thermo-mechanical and durability characteristics. This improvement can be attributed to efficient stress transfer between the fibre and matrix, adequate resin impregnation, and enhanced interfacial bonding resulting from the alkali-treated jute fibres. In contrast, the 20% fibre volume fraction composite recorded the lowest coefficient (0.54) due to insufficient reinforcement content, which limited its load-bearing capability and overall structural performance. Although the 40% fibre volume fraction composite achieved a relatively high closeness coefficient (0.68), its performance was lower than that of the 30% fibre composite [18]. The reduction can be associated with increased fibre crowding, resin starvation, and the formation of voids, which adversely affected composite consolidation and mechanical efficiency. The error bars indicate the standard deviation obtained from repeated experimental measurements, demonstrating good repeatability and consistency of the results. Overall, the optimization analysis confirms that a 30% jute fibre volume fraction provides the optimum balance between reinforcement effectiveness and matrix continuity, making it the most suitable configuration for sustainable structural applications. The findings demonstrate the effectiveness of TOPSIS as a multi-criteria decision-making tool for selecting the best-performing natural fibre composite based on multiple thermo-mechanical performance indicators [19].
9. THERMOGRAVIMETRIC ANALYSIS (TGA)
Figure 14 illustrates the thermogravimetric degradation behavior of jute fibre reinforced polymer (JFRP) composites containing 20%, 30%, and 40% fibre volume fractions. All composite formulations exhibited a similar degradation pattern characterized by distinct stages associated with moisture removal, decomposition of lignocellulosic constituents, epoxy matrix degradation, and residual char formation. In the initial temperature region (50–120°C), a slight reduction in weight was observed for all specimens due to the evaporation of physically absorbed moisture and volatile compounds present within the natural fibres. The weight loss in this stage was relatively small, indicating effective moisture removal during the fibre drying process prior to composite fabrication. The second degradation stage occurred between approximately 120°C and 350°C and was primarily attributed to the thermal decomposition of hemicellulose and partial degradation of cellulose constituents present in the jute fibres. During this stage, the composites exhibited a gradual reduction in mass as the less thermally stable components of the natural fibres began to degrade. The onset degradation temperature was slightly higher for the 30% fibre composite, indicating improved resistance to thermal decomposition. A significant decline in weight retention was observed in the third degradation stage (350–500°C), corresponding to the decomposition of cellulose, lignin, and the epoxy matrix. This region represented the major thermal degradation phase of the composite system. Among the tested formulations, the 30% fibre volume fraction maintained the highest weight retention throughout this stage, demonstrating enhanced thermal stability. The improved performance can be attributed to stronger fibre–matrix interfacial bonding, reduced defect concentration, and the formation of a more compact composite structure that delayed heat-induced degradation. Beyond 500°C, the degradation rate decreased considerably, resulting in the formation of a stable carbonaceous char residue. The residual char yield serves as an important indicator of thermal resistance and flame-retardant behaviour. The 30% fibre composite exhibited the highest residual weight at elevated temperatures, suggesting superior char-forming capability and greater resistance to thermal breakdown. The enhanced char formation acts as a protective barrier that restricts heat transfer and slows further degradation of the composite. The 20% fibre composite exhibited the lowest thermal stability due to insufficient reinforcement content and lower char yield [20]. Conversely, although the 40% fibre composite demonstrated improved thermal resistance compared with the 20% formulation, its performance remained lower than that of the 30% fibre composite. This behaviour may be attributed to increased fibre agglomeration, non-uniform resin distribution, and localized void formation at higher fibre loadings, which accelerate thermal decomposition. Overall, the TGA results indicate that the incorporation of alkali-treated jute fibres significantly enhances the thermal performance of epoxy composites [21]. Among the investigated formulations, the 30% fibre volume fraction exhibited the optimum thermal behaviour, characterized by a higher onset degradation temperature, improved thermal stability throughout the decomposition process, and greater residual char yield. These findings are consistent with the mechanical and multi-objective optimization results, confirming that the 30% JFRP composite provides the most balanced combination of thermo-mechanical properties for sustainable structural applications [22].
Thermogravimetric analysis (TGA) curves of JFRP composites with different fibre volume fractions.
10. CONCLUSION
This study investigated the thermo-mechanical behavior and multi-objective optimization of jute fibre reinforced polymer (JFRP) composites fabricated using the hand lay-up technique. The results demonstrate that fibre volume fraction and alkali surface treatment significantly influence the mechanical and thermal performance of the composites. Mechanical testing showed that tensile and flexural strengths improved with increasing fibre content up to an optimal range of approximately 35–40%, beyond which a decline in performance was observed, likely due to reduced fibre wetting and increased agglomeration. Alkali-treated composites exhibited better mechanical performance compared to untreated samples, which is attributed to improved fibre–matrix interaction as evidenced by SEM observations. Thermal analysis using TGA indicated an increase in degradation temperature for treated composites, confirming improved thermal stability under the investigated conditions. The Response Surface Methodology (RSM) model demonstrated good agreement with experimental results (R2 > 0.95), and ANOVA analysis confirmed the statistical significance of key parameters, particularly fibre volume fraction and treatment concentration. The optimization study identified an optimal combination of process parameters (approximately 35–40% fibre fraction and moderate alkali treatment), which provided a balanced improvement in mechanical properties and thermal stability while maintaining relatively low density. Validation experiments showed that the predicted and experimental results were in close agreement, with deviations below 5%, indicating the reliability of the developed model. Overall, the findings suggest that JFRP composites have potential for lightweight structural and semi-structural applications where moderate strength and thermal resistance are required. However, the results are limited to the specific materials, processing conditions, and parameter ranges considered in this study. Further investigations on long-term durability, environmental effects, and advanced reinforcement strategies are necessary to fully assess their applicability in real-world conditions.
11. DATA AVAILABILITY
No data was used for the research described in the article.
12. BIBLIOGRAPHY
- [1] KHAN, A., AL-KAABI, K., AL-MAADEED, M.A., “Hybrid natural fiber reinforced polymer composites: A review on mechanical and thermal properties”, Materials Today. Communications, v. 35, pp. 105489, 2023.
-
[2] DENNISON, M.S., KIRUBANIDHI JEBABALAN, S., SAMRAJ, A., et al., “Biodegradable electronic materials for promoting sustainability in next-generation electronics - a comprehensive review”, Discover Materials, v. 5, n. 1, pp. 182, 2025. doi: https://doi.org/10.1007/s43939-025-00381-w.
» https://doi.org/10.1007/s43939-025-00381-w - [3] ASTM International. (2018). ASTM D256-18: Standard Test Methods for Determining the Izod Pendulum Impact Resistance of Plastics West Conshohocken, PA, USA: ASTM International.
-
[4] ÖZYER, T., YILMAZ, T., KAYA, M., et al., “Evaluation of jute-glass ratio effects on the mechanical, thermal, and morphological properties of PP hybrid composites for sustainable automotive applications”, Polymers, v. 17, n. 24, pp. 3335, 2025. doi: https://doi.org/10.3390/polym17243335. PubMed PMID: 41471010.
» https://doi.org/10.3390/polym17243335 - [5] SARKER, M.A.H., RAHMAN, M.M., ISLAM, M.A., et al., “Mechanical and morphological characterization of hybrid natural fiber epoxy composites”, Polymer Engineering and Science, v. 6, n. 3, pp. e70016, 2025.
-
[6] PRAVEENA, B.A., RAMESH, M., SURESH, S., et al., “Mechanical and morphological evaluation of jute fiber reinforced epoxy composites for structural applications”, Fracture and Structural Integrity, v. 20, n. 76, pp. 1–16, 2026. doi: https://doi.org/10.3221/IGF-ESIS.76.01.
» https://doi.org/10.3221/IGF-ESIS.76.01 -
[7] RAMAN, A.K., KUMAR, S., RAJENDRAN, S., et al., “Morphological and mechanical evaluation of epoxy hybrid composites reinforced with banana and jute cellulose”, Journal of Mechanical Science and Technology, v. 40, pp. 455–461, 2026. doi: https://doi.org/10.1007/s12206-025-1237-7.
» https://doi.org/10.1007/s12206-025-1237-7 -
[8] KANAGINAHAL, G.M., SHAHAPURKAR, K., KAKKAMARI, P., et al., “Jute fiber and its composites: Processing, properties, and applications”, Journal of Natural Fibers, v. 23, n. 1, pp. 2635010, 2026. doi: https://doi.org/10.1080/15440478.2026.2635010.
» https://doi.org/10.1080/15440478.2026.2635010 - [9] RAMESH, M., PALANIKUMAR, K., HEMACHANDRA REDDY, K., “Mechanical and thermal behavior of natural fiber reinforced epoxy composites: A review”, Composite Structures, v. 320, pp. 117225, 2024.
- [10] KUMAR, R., SINGH, V., “Effect of alkali treatment on jute fiber epoxy composites for structural applications”, Materials Today: Proceedings, v. 72, pp. 2100–2106, 2024.
- [11] DAS, S., PAUL, A., GHOSH, S.K., “Influence of fiber loading on mechanical performance of jute reinforced polymer composites”, Journal of Materials Research and Technology, v. 28, pp. 4560–4572, 2024.
-
[12] SOMSOLE, L.N., THEJASREE, P., NARASIMHAMU, K.L., et al., “Experimental investigation and optimization of epoxy composites reinforced with jute fiber and alumina using the Jaya-ANFIS approach”, Scientific Reports, v. 15, n. 1, pp. 30462, 2025. doi: https://doi.org/10.1038/s41598-025-16587-0. PubMed PMID: 40830582.
» https://doi.org/10.1038/s41598-025-16587-0 - [13] PATEL, H., SHAH, D., “Optimization of process parameters for natural fiber composites using response surface methodology”, Materials Research Express, v. 10, n. 8, pp. 085302, 2023.
- [14] SINGH, T., GANGIL, B., PATNAIK, A., et al., “Surface treatment effects on natural fiber reinforced epoxy composites: A review”, Journal of Reinforced Plastics and Composites, v. 42, n. 9–10, pp. 389–405, 2023.
-
[15] MURUGAN, A., BARIK, D., FAISAL, R.S., et al., “Process parameter optimization for enhanced mechanical and thermal properties of kenaf/jute hybrid composites using grey fuzzy logic”, Scientific Reports, v. 15, n. 1, pp. 36221, 2025. doi: https://doi.org/10.1038/s41598-025-20268-3. PubMed PMID: 41102322.
» https://doi.org/10.1038/s41598-025-20268-3 -
[16] MURUGAN, A., BARIK, D., FAISAL, R.S., et al., “Optimization of tribo-mechanical properties of kenaf/jute-SiC hybrid composites using integrated grey-fuzzy approach”, Scientific Reports, v. 15, n. 1, pp. 26205, 2025. doi: https://doi.org/10.1038/s41598-025-11340-z. PubMed PMID: 40684022.
» https://doi.org/10.1038/s41598-025-11340-z -
[17] KUMAR, S., LAKSHMAIYA, N., RAO, P.U.M., et al., “Synergistic enhancement of jute fiber epoxy composites using hybrid nano-silica and graphene”, Results in Engineering, v. 21, pp. 108603, 2025. doi: https://doi.org/10.1016/j.rineng.2025.108603.
» https://doi.org/10.1016/j.rineng.2025.108603 -
[18] VIJAYALAKSHMI, P., SATHISHKUMAR, S., VIJAYARAJ, M., et al., “Multiobjective optimization of the mechanical characteristics of hybrid fibre-reinforced”, Polymer Composites, v. 2, pp. 277–295, 2025. doi: https://doi.org/10.1007/978-981-96-4632-6_20.
» https://doi.org/10.1007/978-981-96-4632-6_20 -
[19] PEREIRA JUNIO, R., FERREIRA FONTES, J.C., SILVA, D.S., et al., “Mechanical characterization of jute fiber-reinforced composites manufactured via Digital Light Processing (DLP)”, Journal of Materials Research and Technology, v. 37, pp. 1552–1578, 2025. doi: https://doi.org/10.1016/j.jmrt.2025.06.118.
» https://doi.org/10.1016/j.jmrt.2025.06.118 -
[20] DEWANGAN, R.K., “Multi-criteria optimization of mechanical performance of jute–glass–carbon fiber-reinforced hybrid polymer composites using ANOVA, AHP-TOPSIS, and RSM”, Mater. Proc., v. 26, pp. 18, 2025. doi: https://doi.org/10.3390/materproc2025026018.
» https://doi.org/10.3390/materproc2025026018 -
[21] HABIB, A., ISLAM, M.A., HOSSAIN, M.T., et al., “Recent developments in the modification and fabrication of jute fibre-reinforced composites for structural applications”, Discover Sustainability, v. 6, n. 1, pp. 1107, 2025. doi: https://doi.org/10.1007/s43621-025-01785-7.
» https://doi.org/10.1007/s43621-025-01785-7 -
[22] LAKSHMI NARAYANA, S., GOPALAN, V., “Mechanical characterization of particle reinforced jute fiber composite and development of hybrid Grey-ANFIS predictive model”, Journal of Natural Fibers, v. 20, n. 1, pp. 2167033, 2023. doi: https://doi.org/10.1080/15440478.2023.2167033.
» https://doi.org/10.1080/15440478.2023.2167033