Abstract
Abstract This paper evaluates the performance of a highly eco-efficient low-cement concrete incorporating Basic Oxygen Furnace slag (BOFS) as a raw material. The BOFS was processed to obtain fine and coarse powders, with the mix design based on a modified Andreassen method to enhance particle packing at the paste level. This approach resulted in concretes with a cement consumption of only 86.6 kg·m-3. The BOFS concretes were assessed through water absorption, ultrasonic pulse velocity, forced resonant frequency, modulus of elasticity, compressive strength, tensile strength, and pore system analysis. Additionally, electrical resistivity and accelerated carbonation tests were conducted. At 28 days, the BOFS concrete achieved a compressive strength of 35.1 MPa, corresponding to a cement intensity of 2.47 kg·m-3·MPa−1, with substantial strength gains at later ages. Despite its relatively low electrical resistivity due to the iron content, the BOFS concrete exhibited a dense microstructure (void index of 5.5% and ultrasonic pulse velocity of 4276 m/s) and remained stable under high-temperature water immersion. The optimized particle packing contributed to high mechanical performance and promising durability, as evidenced by the low carbonation depth (less than 10 mm in 120 days under 8% CO2). These findings demonstrate that highly eco-efficient BOFS concrete can achieve durability comparable to conventional Portland cement-based concretes. This study reinforces the potential of BOFS as a sustainable alternative, promoting circular economy practices and reducing the environmental footprint of the construction industry.
Keywords:
low-cement concrete; basic oxygen furnace slag; steel slag aggregates; supplementary cementitious material; durability
Resumo
Resumo Este artigo avalia o desempenho de um concreto de baixo teor de cimento altamente ecoeficiente, incorporando escória de Convertedor a Oxigênio (BOFS) como matéria-prima. A BOFS foi processada para obter pós finos e grossos, com o traço do concreto baseado em um método Andreassen modificado para melhorar o empacotamento de partículas no nível da pasta. Essa abordagem resultou em concretos com um consumo de cimento de apenas 86,6 kg·m-3. Os concretos com BOFS foram avaliados por meio de testes de absorção de água, velocidade de pulso ultrassônico, frequência ressonante forçada, módulo de elasticidade, resistência à compressão, resistência à tração e análise do sistema de poros. Além disso, foram realizados testes de resistividade elétrica e carbonatação acelerada. Aos 28 dias, o concreto com BOFS atingiu uma resistência à compressão de 35,1 MPa, correspondendo a uma intensidade de cimento de 2,47 kg·m−3·MPa−1, com ganhos substanciais de resistência em idades posteriores. Apesar da relativamente baixa resistividade elétrica devido ao teor de ferro, o concreto com BOFS apresentou uma microestrutura densa (índice de vazios de 5,5% e velocidade de pulso ultrassônico de 4276 m/s) e permaneceu estável sob imersão em água a alta temperatura. O empacotamento otimizado das partículas contribuiu para um alto desempenho mecânico e uma durabilidade promissora, evidenciada pela baixa profundidade de carbonatação (menos de 10 mm em 120 dias sob 8% de CO2). Esses resultados demonstram que o concreto com BOFS, altamente ecoeficiente, pode alcançar uma durabilidade comparável à dos concretos convencionais à base de cimento Portland. Este estudo reforça o potencial da BOFS como uma alternativa sustentável, promovendo práticas de economia circular e reduzindo a pegada ambiental da indústria da construção civil.
Palavras-chave:
concreto de baixo teor de cimento; escória de aciaria; agregados de escória de aço; material cimentício suplementar; durabilidade
1 INTRODUCTION
The construction industry is responsible for a large part of the worldwide consumption of raw materials. Two essential supplies for this sector are Portland cement and aggregates. The cement industry is the third-largest industrial energy consumer and contributes to approximately 7% of global anthropogenic CO2 emissions [1], [2]. In 2014, the Brazilian construction sector consumed 740 million tons of aggregates produced by extractive activities, with high consumption of resources [3]. At the same time, the steel industry generates a high content of residues during the production process [4]. In 2020, Brazil produced 31 million tons of steel, generating around 5 million tons of steel slag [5].
Among these environmental challenges posed by traditional construction materials, the scientific community has been studying and proposing solutions to mitigate the impacts caused by these sectors [6]–[9]. An alternative that stands out is using steel slag to replace cement and/or aggregates in cement-based composites [9], [10]. This strategy is usually associated with three main points: (1) reducing construction costs [11], (2) increasing eco-efficiency and decreasing the carbon footprint compared to conventional concrete [12], and (3) improving the mechanical performance and durability of the matrices [13]. Thus, processed steel slag is an efficient alternative to reduce the consumption of natural aggregates in cement-based composites.
Using steel slag in cement-based composites also faces criticism. Calcium and magnesium oxides and a metallic iron fraction raise concerns as they can cause expansion and cracking [7], [14]–[19]. However, the weathering and metallic separation have been demonstrated to be efficient in stabilizing these oxides [6]–[8], [15]–[18], [20]. Additionally, many works have shown the mechanical and durability benefits of using steel slag powders and aggregates in cement-based composites, where the steel slag concrete achieved better mechanical resistance than the conventional ones [12], [21]–[25].
Despite the environmental benefits of replacing natural construction materials with steel slag, cement consumption in the construction sector remains significant, as are its environmental impacts, which have already been described [1], [2]. Among the alternatives to reduce cement consumption, the association of particle packing models with supplementary cementitious materials (SCM) presents a good performance in producing alternative sustainable building materials.
The use of SCM further enhances the sustainability of concrete. SCMs improve the durability [26]–[28] and reduce the carbon footprint of cement-based composites [2], [29]. Carvalho et al. [30] made a concrete with steel slag as aggregate and SCM with a cement consumption of less than 90 kg.m-3 (Portland cement ASTM Type III). The steel slag concrete achieved a compressive strength of 37 MPa at 28 days using these dosage approaches. These benefits highlight the potential of SCMs to create more sustainable building materials.
Many concerns emerge about using low-cement concretes, especially for structural applications [31]. The concrete properties depend on the amount of hydrated binder, and there is a consensus that the paste volume highly influences the strength of the concrete matrix [32], [33]. This association remains true for conventional concretes since the porosity is more dependent on the paste volume than the matrix of aggregates. However, many studies have demonstrated the benefits of promoting granulometric optimization and using high-strength cement and superplasticizers to obtain low-cement concrete (LCC) [12], [34], [35]. In addition, using effective SCMs improves workability, reduces hydration heat, and improves mechanical and durability performances by cementing properties and filler effects [12], [30], [31], [36]–[38].
The literature has consolidated the steel slag as an alternative to conventional aggregates in concrete. However, the applicability of steel slag aggregates and powder in LCCs remains an issue. There is a noticeable knowledge gap regarding the durability of steel slag LCCs and their eco-efficient composites, especially in later ages. Thus, this work addresses this gap by thoroughly assessing the physical, mechanical, and durability performances of steel slag LCC (produced with under 86 kg/m3 cement consumption). The novelty and relevance of the present research lie in the evaluation of steel slag LCC’s accelerated carbonation (over periods of up to 120 days) and the long-term assessment of its mechanical behavior (up to 800 days), providing valuable insights to support the potential use of steel slag in LLCs.
2 MATERIAL AND METHODS
2.1 Materials
An ASTM Type III equivalent cement, identified in Brazil as CP-V (NBR 16697 [39]), was used. The producer reported the primary characterization of the cement (Table 1). This cement type was selected since it has a reduced content of SCMs in its composition (95-100% clinker, 0-5% limestone filler). The admixture adopted was a superplasticizer (SP) based on polycarboxylate (Power-flow4000, MC Bauchemie) as a dispersant.
A regional quartz river sand from Minas Gerais was used as reference fine aggregate, and gneiss aggregate was used as reference coarse aggregate. The steel slag aggregates, and the steel slag powder used as SCM were produced using a basic-oxygen furnace (BOF) slag from Minas Gerais, Brazil. This material was received and stored in the yard of the Laboratory of Civil Construction Materials of the Federal University of Ouro Preto (LMC), where it was subjected to weathering in piles of approximately 2 m high through natural wetting and drying cycles for four years to stabilize and reduce the expansion potential [6]. Table 2 shows the chemical compositions of the aggregates obtained using X-ray fluorescence (XRF). The mineralogical characterization of BOF slag was obtained through X-ray Diffraction (XRD), using the Anton Paar XRDynamic 500 equipment, with CuKα tube, 40 kV voltage, 50 mA current, rotation speed of 30 rpm, 2θ ranging from 10-70° with a step size of 0.005 °/s. For quantitative analysis and determination of the mineralogical phases present in each of the materials, the Rietveld refinement method was employed, using the XRD Analysis software and the International Center for Diffraction Data (ICDD, PDF5+) database, presented in Table 3 and Figure 1.
Figure 2 shows the morphology of the aggregates (Coleman NTB-3ª stereoscope with an HDCE X5 camera and ScopeImage 9.0 software for image processing). The gneiss gravel has a characteristic lamellar shape, and the BOF slag has a cubic/rounded shape. The images can also identify the uniformity of the gneiss gravel surface. The BOF slag presents a rough surface.
The BOF aggregates were produced comprising (1) dry magnetic separation using a magnetic roll (Inbras CC Ø12 x 12, 5000 Gauss intensity); (2) comminution of the material retained in the 25 mm sieve in a jaw crusher (Retsch BB200). The BOF and conventional aggregates were subjected to sieving to obtain an identical particle size distribution curve. The equivalent granulometry for both types of aggregates (BOF and conventional) aids in producing physically similar concretes to evaluate the influence of the material's characteristics on their properties. This processing methodology has been well-established in the literature, with various research studies adopting [40]–[43] this protocol for different sources of steel slag, achieving good stability and low resource consumption during the process. Figure 3 presents the granulometry of fine and coarse aggregate. Moreover, Table 4 shows the physical characteristics of the conventional aggregates and the BOF slag.
- Particle size distribution of the fine aggregates (fine BOF and quartz river sand) and coarse aggregates (coarse BOF and gneiss gravel)
The powders were produced according to the methodology of Carvalho et al. [17]. Two powders with different particle size distributions were produced: (1) the coarse BOF slag powder, obtained by a low-efficiency grinding program using a laboratory ball mill (Marconi, MA500, 200 rpm, 180 minutes, stainless steel jar and balls); and (2) the fine BOF slag powder, produced from the coarse powder by additional grinding in a high-efficiency program, using a planetary ball mill (Retsch, PM100, 400 rpm, 45 minutes, ZrO2 jar and balls ). Figure 4 presents the particle size distributions of the coarse and fine BOF slag powders and the cement used to produce the concretes evaluated. The particle size distribution curves were obtained using the laser granulometry technique (Bettersizer 2000 particle size analyzer, isopropyl alcohol as dispersing medium). The BOF slag powders reached two different particle size distribution ranges: greater and smaller than the Portland cement, respectively coarse and fine BOF slag powder. Such granulometry aids in providing a denser packing.
2.2 Mix design of the LCCs
The proportions of the materials used for the concrete mixture were studied by Carvalho et al. [30] and based on the modified Andreassen method. This method considers an optimal particle size distribution curve, which aims to achieve a proportioning between the materials with the lowest possible pore content (theoretically 0) by analyzing particle diameters. Table 5 presents the components and proportioning. The studied mixtures aim to consume the maximum content of recycled materials, reaching up to 95% by volume of solids, with a cement consumption of 86.6 kg.m-3.
The mixtures had an optimum water/solids ratio of 0.23 ± 0.01 in concretes with conventional aggregates and 0.24 ± 0.01 in concretes with slag aggregates, using 1% SP by mass of fines (cement + powders). The fine aggregates were oven-dried at 105 ºC for 24 hours, and the coarse aggregates were used in the saturated dry surface condition. These conditions led to a high packing density of the prototypes, resulting in a significant decrease in voids and less water consumption.
2.3 Production of the LCCs
The mix homogenization proceeded in steps of 30 seconds, obeying the following order: (1) fine aggregate plus steel slag fines; (2) addition of cement; (3) addition of the coarse aggregate. After homogenization, 50% of water containing the total amount of SP was added to the system for an average mixing time of 2 minutes. Afterward, the remaining water was added carefully to achieve the specified consistency index of 30 ± 1 cm. The consistency index test was carried out following the method NBR 13276 [42] (consistency table, 30 drops). The consistency was fixed for both concretes to maintain the rheological characteristics regardless of the aggregates' physical variables.
The concrete production process had a maximum of 1 hour per line, avoiding any change due to the cement setting. For each mixture, 78 cylindrical specimens measuring ∅5×10 cm were produced. The specimens were compacted in 3 layers, applying 10 strokes per layer, and cured until testing age in a humid chamber with controlled humidity and temperature (95%, 23±2 °C).
2.4 Physical and mechanical characterization of the hardened concretes
Table 6 shows the standard methods, the number of repetitions, and the testing age used to characterize the concretes. Mechanical characterizations were performed at different ages to describe the behavior over long periods.
Specific gravity, water absorption, and void ratio were measured through the hydrostatic weighing method (NBR 9778 [44]). The void index is defined as the ratio of the volume of permeable pores to the volume occupied by a solid sample. The Proceq TICO apparatus (54 kHz longitudinal pulse transducers) was used for the ultrasonic pulse velocity. The UPV test was obtained by direct transmission since both sample faces were available; this transmission type is considered the most reliable method. The forced resonant frequency l was performed on the Erudite MKII Resonancy Frequency Test System equipment (C.N.S. Electronics). The modulus of elasticity of LCC was calculated using the results of ultrasonic pulse velocity and resonant frequency, following, respectively, ASTM C597 [47] and ASTM C215 [48].
A hydraulic press (EMIC DL 20000) with a load cell of 200 kN and a machine loading speed of 0.3 MPa/s was used to conduct the mechanical tests (compressive and tensile strength). The LCC samples were tested for compressive strength until 800 days, remaining in a humid chamber with controlled humidity and temperature (95%, 23±2 °C) until testing age. It is widely known that tensile strength correlates with compressive strength results. The NBR 6118 [54] defines a standardized equation for this purpose. Considering laboratory limitations and resource optimization, the tensile strength for the 800 days was obtained by calculations. For the other ages, the tensile strength was measured experimentally.
The analysis of the pore system proposed by Mendes [53] maps and quantifies the number of pores identified in a section. The parameters obtained in this test were pore size distribution and pore content in the section. The ∅5×10 cm specimens were cross-cut using a diamond saw in wet cutting. Subsequently, the faces were polished with sandpaper of 80 and 400 grits. Then, the area was painted with a black brush, and the pores were filled with a fine white powder, creating a high contrast between the pores and the matrix. The sections were digitally registered (HP Scanjet G4050 scanner, resolution of 2400 dpi) and treated in image editing software. The sections were transformed into black-and-white images and processed by an algorithm in the Scilab® software to count white and black pixels. The algorithm provides the average pore radius and the porosity in the cross-sections. The measurement accuracy is 20 μm (defined by the scanner resolution). Figure 5 shows the initial and final images of one of the intermediate sections of concrete used in the surface porosity test.
- Initial and treated images of the cross-sections of CCA and CBSA specimens in the surface porosity test. (a) CCA: natural cross-section (left) and treated image highlighting pores (right); (b) CBSA: natural cross-section (left) and treated image highlighting pores (right).
2.5 Durability performance
Table 7 shows the properties and standard methods used to evaluate durability. The tests were performed at 28 days of age.
The accelerated carbonation test was carried out using the carbonation chamber SCO 26H ShelLab®. The specimens were covered with a Silver Tape® layer along the length and at the base for this test. The set, specimen, and tape were sealed externally with an additional layer of paraffin, exposing only the upper face to the CO2-rich atmosphere to achieve a single-way carbonation front (from the exposed face, along the 10 cm height of the specimen) [58].
The carbonation chamber atmosphere was set at 8% CO2 concentration, relative humidity of 50%, and temperature of 25 ºC, according to the methodology used by Andrade et al. [58]. The exposure times were 64 and 120 days.
A colorimetric method was used to determine the carbonation depth using a 1% phenolphthalein solution, according to the requirements of the CPC-18 standard [59]. For this procedure, the specimen is fractured along its length. After the fracture, the phenolphthalein solution was sprinkled on the exposed surface, and the carbonation depth was determined by measuring the thickness of the uncolored region (carbonated – low pH) on the top of the specimens, which differs from the pink-colored region (non-carbonated - high pH).
2.6 Eco-efficiency evaluation
The LCC eco-efficiency evaluation used the parameters waste consumption and binder intensity (bi), proposed by Damineli et al. [28]. Cement intensity relates binder consumption to a concrete performance. For the present work, the performance parameter chosen was compressive strength. Equation 1 describes the calculation of bi, where b is the total binder consumption in kg.m-3 (Portland cement), and p is the performance achieved (compressive strength at 28 days, 90 days, and 800 days).
Waste consumption was calculated through the mix design, considering the total mass of all BOF slag fractions (fine powder, coarse powder, fine aggregate, and coarse aggregate) that could be incorporated to produce 1 m3 of the proposed LCC.
3 RESULTS AND DISCUSSION
3.1 Physical and mechanical characterization of the LCCs
3.1.1 Density and porosity
The density of the LCCs was 3.1 g/cm3 for the CBSA and 2.6 g/cm3 for the CCA. The incorporation of BOF aggregates enhances 19% of the property. This result was already expected since the steel slag comprises a high content of metallic oxides (as shown in Table 3). Both LCCs have a density more elevated than the usual for normal concretes (NBR 6118 [54]), indicating the production of a low porosity matrix.
Figure 6 shows the void index and water absorption results. The LCC presented water absorption lower than reported in the literature for conventional concretes fabricated with high porosity aggregates, such as lightweight aggregates and concrete recycled aggregates [12,30]. The water absorption of LCC is equivalent to concretes fabricated with a total replacement of aggregates by steel slag with a cement consumption of approximately 350 kg.m-3 [58]. Thus, these results indicate that a reduction in cement consumption is possible when accompanied by optimal proportioning with SCM materials and a packing approach.
Replacing gneiss aggregate with BOF aggregate led to a reduction in the water absorption parameter due to the morphology of the aggregates. The cubic/rounded shape of the BOF aggregate (Figure 1) provides greater mobility to the cementitious fresh matrix and a better capacity to occupy voids, promoting a higher packing density. Additionally, the gneiss aggregates have a lamellar shape (Figure 2), contributing to a more significant water accumulation in their vicinity and a higher porosity [28] .
The void index test involves a boiling stage for the sample, introducing a harmful situation for the composites. In this same condition, the CCA concrete specimens showed cracks on the top, while the CBSA specimens remained intact, as shown in Figure 7. The cracks can be related to an expansion process verified by the increased diameters of the CCA specimens. The BOF slag aggregate provided a sound interfacial transition zone and a greater interlocking with the paste due to its porous and rough surface, preventing crack formation and propagation.
- (a) Concrete with conventional aggregates (CCA) after 5 hours submerged in water at 100ºC (b) Concrete with BOF slag aggregates (CBSA) after 5 hours submerged in water at 100ºC.
Table 8 shows the pore ratio and average pore radius of the evaluated concretes according to the method proposed by Mendes [53]. The pore ratio of both concretes, which is less than 1%, indicates that the concretes used in this study have low surface porosity. Pessôa et al. [60] evaluated the surface porosity using scanner images and concluded that class C30 concretes have good results compatibility between the methods. This work indicated a 1.6% surface porosity for conventional 30 MPa concretes [61], twice higher than the CBSA.
Figure 8 shows the pore size and distribution. There is a higher percentage of pores in both concretes whose size is between 20 - 50 µm, confirming the matrix's high compactness and homogeneity. The replacement of natural aggregates by BOF slag aggregates enhanced the matrix refinement, with 80.99% of the pore volume of CBSA being less than 250 µm, compared to 64.54% for CCA. As is widely known, a greater pore refinement indicates better durability.
Carvalho et al. [62] evaluated the pore size distribution (analysis of the pore system proposed by Mendes [53]) of cement-based composites produced with steel slag powder (25 wt.% replacement of Portland cement, cement consumption of 389.6 kg.m-3). The authors reported that the lowest pore size comprised in the matrix was inferior to 150 μm; also, the steel slag powder (D90 = 47.45 μm) presented a potential to refine the matrix pore structure (66% of pores <150 μm compared to 51% for REF). In this sense, despite the proposed LCCs having a low cement consumption (86.7 kg.m-3), the optimized packing strategy produced composites with higher content of small diameter pore size compared to the literature.
The porosity results presented in Figure 8 were consistent with the void index and water absorption test. Using a high volume of fines with an adequate particle size distribution aligned with the mixing and molding methodology implied a high compactness, resulting in the pores' refinement. Such refinement contributes positively to physical, mechanical, and durability performances. Additionally, this reinforced the competence of the slag fines as supplementary cementitious material, which has enhanced the matrix performance in association with BOF slag aggregates. Based on the findings, incorporating BOF slag as aggregates in LCC results in a lower permeable porosity (Figure 6), leading to a matrix characterized by reduced-sized unconnected pores (Table 8 and Figure 8).
3.1.2 Elasticity Modulus by ultrasonic pulse velocity and resonant frequency
Figure 9 shows the ultrasonic pulse velocity (UPV), resonant frequency and elasticity modulus (calculated by both procedures) of the low-cement concretes. The UPV results are consistent with the study of Pang et al. [22], who stated that increasing the replacement rate of aggregates for steel slag increases the UPV of the concretes. The porosity and the way the voids are connected directly impact the UPV in the matrix [37].
- Results obtained in the UPV test, resonant frequency and modulus of elasticity calculated by both methods
The UPV values were between 3500-4500 m/s, indicating that both mixtures are uniform, cohesive, and compact [23], [63]. The result demonstrates the effectiveness of the packing and molding methodology. The BOF aggregates enhanced the LCC performance. The CBSA has a UPV 7% higher than the CCA. According to the literature [23], [63], CBSA is classified as excellent and CCA as good. Despite the low cement content, the CBSA presents a UPV result higher than the usual UPV reported in the literature for steel slag concretes [28], [58]. This result indicates that high replacements of Portland cement by BOF powder using a packing approach do not incur any detriment.
The resonant frequencies of CCA and CBSA were almost identical, which differs from UPV results. According to Sales [64], the resonant frequency increases when the density increases and the aggregate porosity decreases. The slag aggregate has a higher density but is more porous due to the steelmaking process, which could explain the slight difference in resonant frequency between the two concretes.
As expected, results for the modulus of elasticity calculated by the UPV and resonant frequency methods were different but consistent. CCA and CBSA have a high modulus of elasticity, indicating high cohesion and uniformity. Both concretes corresponded to class C50 concretes produced with granite aggregates, according to Brazilian standard NBR 6118 [54]. The results indicate that the CBSA has a slightly higher modulus of elasticity. CCA and CBSA have a physical similarity due to the identical proportioning and curing, which confirms that the elastic modulus and porosity are directly related to the nature and characteristics of the aggregates. A greater modulus of elasticity implies better mechanical and durability performance, as this parameter is directly related to the compactness and cohesion of the matrices. In both procedures, the modulus of elasticity of CBSA was higher.
3.1.3 Compressive and tensile strength
Figure 10 shows the compressive strength results at 7, 28, 90, and 800 days. CCA and CBSA reached the strengths prescribed for structural concretes [54], despite the low cement content, corresponding to only 3.47% of the volume of solids.
In the early ages (7 days), CBSA had a compressive strength 32% weaker than that of CCA. However, beyond this initial period, CBSA rapidly surpassed CCA’s compressive strength, consistently achieving significantly higher strengths. BOFS aggregates are mechanically stronger and have an aspect ratio closer to 1 when compared to gneiss gravel (lamellar particles, Figure 1). Their rough and porous surfaces enable better adhesion and interlocking with the cement paste, providing a sound and stronger interfacial transition zone. In addition, their ability to reserve water for long-term hydration (autogenous curing) contributes to a higher hydration degree of the cement particles over time.
This hydration mechanism is closely tied to the constituent aggregate. The rough surface of the BOF slag aggregate promotes a gradual release of water from its pores and irregularities. This characteristic facilitates the hydration of fines at later ages and better accommodation between the paste and aggregates, agreeing with the literature [65]. This increases uniformity and compactness, justifying better mechanical performance [37].
The notable increase in the compressive strength observed in both concretes at ages later than 28 days can be attributed to the cementing action of the BOF slag powder. Materials rich in C2S exhibit cementing properties but with delayed action. The enhanced availability of water for continuous hydration, promoted by the BOFS aggregates, amplified the contribution of BOF slag powder in the compressive strength at later ages [66], [67]. Consequently, the performance of CBSA (35.05 MPa) stands out, showcasing a strength about 40% higher than that of CCA, despite utilizing a 96% consumption of recycled materials.
At 90 and 800 days of age, both specimens achieved even greater compressive strengths compared to 28 days and with an upward linear behavior. The BOF slag presents less than 30% amorphous content (Table 3). Also, as the prominence of the cementitious action at 90 days of age is not usual, such results may indicate a pozzolanic action and consistent long-term hydration [66]. Generally, the steel slag powder is associated with a cementitious action inferior to that of the Portland cement, with a lower contribution to compressive strength [68], [69]. Thus, this indicates that the packing strategy was efficient in enhancing the contribution of BOF slag in the mechanical performance of the composite.
Regarding the literature, Santamaria et al. [70] evaluated steel slag concrete (total replacement coarse fraction and partial replacement fine fraction) with 350 kg.m-3 cement consumption (w/c 0.51), achieving 69 MPa at 28 days and 71 MPa at 90 days. Biskri et al. [71] produced concrete with a cement consumption of 470 kg.m-3 (w/c 0.3, 10 wt.% silica fume by cement) and replacement of coarse aggregates with steel slag, reaching a compressive strength of 74.5 MPa to 86 MPa at 360 days. Thus, the packing strategy allowed compressive strength compatible with the literature despite the low cement content (86.6 kg.m-3) of CCA and CBSA.
Figure 11 presents the results of the tensile strength tests by diametrical compression. In the early stages, the tensile strength in diametrical compression was higher in CCA. At 28 days, both concretes exhibited increased strength, with CBSA standing out. The most significant strength increase from 7 to 28 days observed in CBSA may be attributed to greater hydration of the BOFS powders facilitated by the water released by the BOFS aggregates, owing to the morphology interactions of coarse aggregates at the interfaces already explained in the compressive strength result.
At 90 days of age, both specimens achieved higher tensile strength compared to 28 days, and also with a linear increase. Although the values appear similar to the compression results, a prominent standard deviation was observed, as shown in Figure 10, with CCA standing out at 28 days. The morphology of the gneiss gravel contributes to this phenomenon since its lamellar shape (Figure 2) does not provide homogeneity, implying a variability of results according to its disposition inside the matrix.
3.2 Durability of the LCCs
3.2.1 Electrical resistivity
The results obtained in the electrical resistivity test were 35.80 Ohm.m for CCA and 36.50 Ohm.m for CBSA. According to the classification of AASHTO [72], both matrices have a high potential for ion penetration since their results were less than 54 Ohm.m and, consequently, a high risk of corrosion of the reinforcement. However, the density, water absorption, UPV, resonant frequency, and porosity results indicated uniformity, cohesion, pore refinement, and compactness. As the penetration of aggressive agents depends directly on the pore structure, there is a discrepancy between the results obtained.
This fact can be explained by the matrix's chemical composition, which greatly influenced the result of the resistivity test. BOF slag presents high levels of metallic iron (21.2%, Table 3), increasing the matrix's electrical conductivity and influencing its electrical resistivity result. The AASHTO [72] regulation considers the assessment of concretes completely developed with conventional aggregates, and additional considerations must be made when using recycled materials. In this way, it can be inferred through the correlation of the two tests and the chemical characterization of the materials that the matrix presented low resistivity because of the high electrical conductivity provided by the metallic iron content. The literature has already reported the demand for a particular classification for steel slag composites when electricity is involved. Studies using migration techniques for chloride resistance, such as the ASTM C1202, indicated the influence of the metallic ions content in the results, generating a false negative [73].
Additionally, BOF slag comprised 96.5% solid volumes of CBSA and 32.6% of the CCA. Despite the BOF slag content being almost three times higher for CBSA than CCA, the electrical resistivity is approximately 2% superior. These results revealed that the powder fraction has a more significant influence on the electrical conductivity of the matrix and that the pore refinement suppresses the hazardous effects.
3.2.2 Accelerated carbonation
The carbonation depth of the concretes was evaluated after 64 and 120 days of exposure to a CO2-rich environment, as shown in Figure 12 and Figure 13.
After 64 days of exposure to carbonatation, the CCA presented an average carbonation depth of 2 mm, while the CBSA had a depth of 3 mm. The similarity between the results corroborates the study by Santamaría et al. [70], which exposed conventional concrete specimens and concretes produced using slag aggregates to CO2-rich environments (8%), achieving similar results when used with the phenolphthalein indicator [70].
In the analysis of 120 days of carbonatation exposure, the CCA had a carbonatation depth of 9 mm, while the CBSA had a depth of 6 mm. This difference agrees with the study of Andrade [58], which evaluated concretes with conventional aggregates and BOF slag aggregates after 160 days of exposure to a CO2-rich atmosphere (8%). The concrete with conventional aggregates had a carbonation depth of 21 mm, while the concrete with BOF slag reached a depth of 8mm, both with a cement consumption of around 86.6 kg.m-3.
The remarkable results of accelerated carbonation agree with the voids index, UPV, resonant frequency, elasticity module, and compressive and tensile strengths. Such results consolidate the argument of both specimens' high compactness, low permeability, and high homogeneity. These characteristics enhance the durability of these concretes and contribute to enhance mechanical performance.
In the carbonation evaluation, the difference in performance between CCA and CBSA was not prominent. The differential for achieving such results was using steel slag fines together with an adequate particle size distribution and mixing/molding methodology.
3.2.3 Eco-efficiency
Both LCCs showed promising eco-efficiency results, so increased BOF slag content reduced the cement intensities for all mixtures. Table 9 shows the evaluation of the eco-efficiency of the studied concretes.
The CBSA mixture obtained cement intensity lower than CCA for all ages. For the 28-day results, CBSA cement intensity was 2.47 kg.m-3.MPa-1 while the CCA reached 3.51 kg.m-3.MPa-1. This result was already expected since CBSA presented higher compressive strength results with the same cement consumption (86.6 kg.m-3). However, the cement intensity obtained for both proposed LCCs stands out from the literature. Damineli et al. [74] evaluated a database with a 1585 register, and the minimum observed cement intensity seems to reach a plateau in the 5 kg.m-3.MPa-1 range. Comparing the results with other steel slag concrete found in the literature, Costa et al. [43] evaluated concretes with total replacement of conventional aggregates by BOF slag. For a cement consumption of 310 kg.m-3 the BOF concretes presented a cement intensity of 7.58 kg.m-3.MPa-1, while the conventional one was 13.29 kg.m-3.MPa-1.
Both LCCs evaluated in this study had 86.6 kg.m-3 of cement content. However, only 30% of CCA volume comprises residues (BOF slag), while CBSA allows a higher incorporation (97% of the mixture volume). Consequently, CBSA can incorporate 140% more BOF slag in 1 m3 of LCC produced. These results allowed an indirect assessment of the environmental performance related to BOF slag incorporation. Besides the contribution of LCC in lowering the CO2 emission for the construction sector, replacing conventional aggregates with BOF slag offers an effective and straightforward way to minimize the construction sector's environmental footprint, promoting the production of cleaner concrete.
The mechanical competence of the LCC remains adequate even with the high amount of BOF slag in granular and fine form, despite the low consumption of cement and the total substitution of aggregates in its mixture. The compressive strengths results associated with the lower cement intensity and the greater consumption of residues (more than 95%) indicate that CBSA presents better eco-efficiency results. The results are even better than those obtained by Franco de Carvalho et al. [30] in the previous study, and the long-term performance led to extremely low cement intensities, reaching less than 1 kg.m-3.MPa-1 for 800 days of curing.
4 CONCLUSION
This study successfully assesses the main durability issues of BOF slag LCC with an expanded performance evaluation. The main findings are summarized as follows:
-
The morphological observations of the BOF slag aggregates confirm an adequate aspect ratio for promoting fresh concrete's good packing. Their porosity and rough surfaces promote strong interfacial transition zones and retention of hydration water for long-term autogenous curing.
-
The combination of the aggregate’s particle sizes and cement, coarse, and superfine BOF slag powders promoted an efficient particle size distribution of the solid fraction, leading to a densely packed fresh mixture, as demonstrated by the low water consumption and physical and mechanical characterization of the hardened concretes.
-
The mechanical tests showed a slower strength gain of the LCC containing BOF slag than natural aggregates in initial ages. Despite reaching a lower initial strength, CBSA had a better mechanical performance than CCA for the later ages, achieving compressive strengths of 35.1 MPa for 28 days, 43.9 MPa for 90 days, and 90.93 MPa for 800 days.
-
The extremely low cement consumption (86.6 kg.m-3) associated with high compressive strength values led to cement intensities of 2.47, 1.97 and 0.95 kg.m-3.MPa-1 for 28, 90, and 800 days of curing. The maximum consumption of recycled material was 2976.2 kg.m-3.
-
The results of forced resonant frequency and UPV indicated the effectiveness of the packing density-oriented concrete mix design, suggesting a high cohesion, compactness, and uniformity of the concrete matrix.
-
Except for electric resistivity, due to incompatibility of the test for materials rich in iron-containing minerals, the durability tests showed that the BOF slag LCC concretes evaluated presented results compatible with sound and durable concretes, highlighting the small carbonation depths due to the low porosity.
The results demonstrated that it is possible to produce LCCs with high eco-efficiency performances using BOF slag as supplementary cementitious material and aggregates, through packing techniques, with promising characteristics that point to sound and durable cement-based composites.
5 ACKNOWLEDGMENTS
The authors acknowledge the financial support provided by CAPES, CNPq and FAPEMIG, as well as the infrastructure provided by UFMG and UFOP. The authors acknowledge the following laboratories for the equipment use and technical support: Laboratory for Characterization of Mechanical and Civil Construction Materials – Department of Materials and Construction Engineering - UFMG; Laboratory of Materials for Civil Construction - Department of Civil Engineering - UFOP. We also thank the Research Group on Solid Waste RECICLOS–CNPq for the infrastructure and collaboration.
Financial support:
Data Availability:
How to cite:
6 REFERENCES
-
1 S. Çankaya and B. Pekey, "A comparative life cycle assessment for sustainable cement production in Turkey," J. Environ. Manage., vol. 249, pp. 109362, 2019, http://doi.org/10.1016/j.jenvman.2019.109362
» http://doi.org/10.1016/j.jenvman.2019.109362 - 2 J. Lehne, F. Preston, Innovation in Low-carbon Cement and Concrete, London: Chatham House Report, 2018.
-
3 F. N. Costa and D. V. Ribeiro, "Reduction in CO2 emissions during production of cement, with partial replacement of traditional raw materials by civil construction waste (CCW)," J. Clean. Prod., vol. 276, pp. 123302, 2020, http://doi.org/10.1016/j.jclepro.2020.123302
» http://doi.org/10.1016/j.jclepro.2020.123302 - 4 World Steel Association, Steel’s Contribution to a Low Carbon Future and Climate Resilient Societies, Bruxelas: World Steel Association, 2020.
- 5 IABR, Relatório de sustentabilidade 2019-2020, Rio de Janeiro: IABR, 2020.
-
6 T. Zhang, Q. Yu, J. Wei, J. Li, and P. Zhang, "Preparation of high performance blended cements and reclamation of iron concentrate from basic oxygen furnace steel slag," Resour. Conserv. Recycling, vol. 56, no. 1, pp. 48–55, 2011, http://doi.org/10.1016/j.resconrec.2011.09.003
» http://doi.org/10.1016/j.resconrec.2011.09.003 -
7 D. H. Diniz, J. M. F. de Carvalho, J. C. Mendes, and R. A. F. Peixoto, "Blast oxygen furnace slag as chemical soil stabilizer for use in roads," J. Mater. Civ. Eng., vol. 29, no. 9, pp. 29, 2017, http://doi.org/10.1061/(ASCE)MT.1943-5533.0001969
» http://doi.org/10.1061/(ASCE)MT.1943-5533.0001969 -
8 M. J. Da Silva, B. P. De Souza, J. C. Mendes, G. J. S. Brigolini, S. N. Da Silva, and R. A. F. Peixoto, "Feasibility study of steel slag aggregates in precast concrete pavers," ACI Mater. J., vol. 113, no. 4, pp. 439-446, 2016, http://doi.org/10.14359/51688986
» http://doi.org/10.14359/51688986 -
9 Y. Jiang, T.-C. Ling, C. Shi, and S.-Y. Pan, "Characteristics of steel slags and their use in cement and concrete—A review," Resour. Conserv. Recycling, vol. 136, pp. 187–197, 2018, http://doi.org/10.1016/j.resconrec.2018.04.023
» http://doi.org/10.1016/j.resconrec.2018.04.023 -
10 A. C. P. Martins et al., "Steel slags in cement-based composites: an ultimate review on characterization, applications and performance," Constr. Build. Mater., vol. 291, pp. 123265, 2021, http://doi.org/10.1016/j.conbuildmat.2021.123265
» http://doi.org/10.1016/j.conbuildmat.2021.123265 -
11 D. R. Gonçalves, W. C. Fontes, J. C. Mendes, G. J. Silva, and R. A. Peixoto, "Evaluation of the economic feasibility of a processing plant for steelmaking slag," Waste Manag. Res., vol. 34, no. 2, pp. 107–112, 2016, http://doi.org/10.1177/0734242X15615955
» http://doi.org/10.1177/0734242X15615955 -
12 J. M. Franco de Carvalho, T. V. de Melo, and W. C. Fontes, "J.O. dos S. Batista, G.J. Brigolini, R.A.F. Peixoto, More eco-efficient concrete: an approach on optimization in the production and use of waste-based supplementary cementing materials," Constr. Build. Mater., vol. 206, pp. 397–409, 2019, http://doi.org/10.1016/j.conbuildmat.2019.02.054
» http://doi.org/10.1016/j.conbuildmat.2019.02.054 -
13 N. Palankar, A. U. Ravi Shankar, and B. M. Mithun, "Durability studies on eco-friendly concrete mixes incorporating steel slag as coarse aggregates," J. Clean. Prod., vol. 129, pp. 437–448, 2016, http://doi.org/10.1016/j.jclepro.2016.04.033
» http://doi.org/10.1016/j.jclepro.2016.04.033 -
14 Q. Wang, D. Wang, and S. Zhuang, "The soundness of steel slag with different free CaO and MgO contents," Constr. Build. Mater., vol. 151, pp. 138–146, 2017, http://doi.org/10.1016/j.conbuildmat.2017.06.077
» http://doi.org/10.1016/j.conbuildmat.2017.06.077 -
15 L. V. Fisher and A. R. Barron, "The recycling and reuse of steelmaking slags — A review," Resour. Conserv. Recycling, vol. 146, pp. 244–255, 2019, http://doi.org/10.1016/j.resconrec.2019.03.010
» http://doi.org/10.1016/j.resconrec.2019.03.010 -
16 G. Kang, A. A. Cikmit, T. Tsuchida, H. Honda, and Y. Kim, "Strength development and microstructural characteristics of soft dredged clay stabilized with basic oxygen furnace steel slag," Constr. Build. Mater., vol. 203, pp. 501–513, 2019, http://doi.org/10.1016/j.conbuildmat.2019.01.106
» http://doi.org/10.1016/j.conbuildmat.2019.01.106 -
17 W. Shen, M. Zhou, W. Ma, J. Hu, and Z. Cai, "Investigation on the application of steel slag–fly ash–phosphogypsum solidified material as road base material," J. Hazard. Mater., vol. 164, no. 1, pp. 99–104, 2009, http://doi.org/10.1016/j.jhazmat.2008.07.125
» http://doi.org/10.1016/j.jhazmat.2008.07.125 -
18 I. Z. Yildirim and M. Prezzi, "Geotechnical Properties of Fresh and Aged Basic Oxygen Furnace Steel Slag," J. Mater. Civ. Eng., vol. 27, no. 12, pp. 04015046, 2015, http://doi.org/10.1061/(ASCE)MT.1943-5533.0001310
» http://doi.org/10.1061/(ASCE)MT.1943-5533.0001310 -
19 M. Tafesse, H. K. Lee, A. S. Alemu, H.-K. Kim, and S. Pyo, "On the expansive cracking of a cement matrix containing atomized basic oxygen furnace slag with a metallic iron," Constr. Build. Mater., vol. 264, pp. 119806, 2020, http://doi.org/10.1016/j.conbuildmat.2020.119806
» http://doi.org/10.1016/j.conbuildmat.2020.119806 -
20 P.-Y. Mahieux, J.-E. Aubert, and G. Escadeillas, "Utilization of weathered basic oxygen furnace slag in the production of hydraulic road binders," Constr. Build. Mater., vol. 23, no. 2, pp. 742–747, 2009, http://doi.org/10.1016/j.conbuildmat.2008.02.015
» http://doi.org/10.1016/j.conbuildmat.2008.02.015 -
21 H. Qasrawi, "The use of steel slag aggregate to enhance the mechanical properties of recycled aggregate concrete and retain the environment," Constr. Build. Mater., vol. 54, pp. 298–304, 2014, http://doi.org/10.1016/j.conbuildmat.2013.12.063
» http://doi.org/10.1016/j.conbuildmat.2013.12.063 -
22 B. Pang, Z. Zhou, and H. Xu, "Utilization of carbonated and granulated steel slag aggregate in concrete," Constr. Build. Mater., vol. 84, pp. 454–467, 2015, http://doi.org/10.1016/j.conbuildmat.2015.03.008
» http://doi.org/10.1016/j.conbuildmat.2015.03.008 -
23 S. Saxena and A. R. Tembhurkar, "Impact of use of steel slag as coarse aggregate and wastewater on fresh and hardened properties of concrete," Constr. Build. Mater., vol. 165, pp. 126–137, 2018, http://doi.org/10.1016/j.conbuildmat.2018.01.030
» http://doi.org/10.1016/j.conbuildmat.2018.01.030 -
24 Q. Wang, P. Yan, J. Yang, and B. Zhang, "Influence of steel slag on mechanical properties and durability of concrete," Constr. Build. Mater., vol. 47, pp. 1414–1420, 2013, http://doi.org/10.1016/j.conbuildmat.2013.06.044
» http://doi.org/10.1016/j.conbuildmat.2013.06.044 -
25 L. Mo, F. Zhang, M. Deng, F. Jin, A. Al-Tabbaa, and A. Wang, "Accelerated carbonation and performance of concrete made with steel slag as binding materials and aggregates," Cement Concr. Compos., vol. 83, pp. 138–145, 2017, http://doi.org/10.1016/j.cemconcomp.2017.07.018
» http://doi.org/10.1016/j.cemconcomp.2017.07.018 -
26 A. AlArab, B. Hamad, and J. J. Assaad, "Strength and durability of concrete containing ceramic waste powder and blast furnace slag," J. Mater. Civ. Eng., vol. 34, no. 1, pp. 34, 2022, http://doi.org/10.1061/(ASCE)MT.1943-5533.0004031
» http://doi.org/10.1061/(ASCE)MT.1943-5533.0004031 -
27 I. Y. Hakeem, F. Althoey, and A. Hosen, "Mechanical and durability performance of ultra-high-performance concrete incorporating SCMs," Constr. Build. Mater., vol. 359, pp. 129430, 2022, http://doi.org/10.1016/j.conbuildmat.2022.129430
» http://doi.org/10.1016/j.conbuildmat.2022.129430 -
28 L. C. B. Costa, M. A. Nogueira, H. D. Andrade, J. M. F. de Carvalho, F. P. F. Elói, G. J. Brigolini and R. A. F. Peixoto, "Mechanical and durability performance of concretes produced with steel slag aggregate and mineral admixtures," Constr. Build. Mater., vol. 318, pp. 126152, 2022, http://doi.org/10.1016/j.conbuildmat.2021.126152
» http://doi.org/10.1016/j.conbuildmat.2021.126152 -
29 A. Mohammadi and A. M. Ramezanianpour, "Investigating the environmental and economic impacts of using supplementary cementitious materials (SCMs) using the life cycle approach," J. Build. Eng., vol. 79, pp. 107934, 2023, http://doi.org/10.1016/j.jobe.2023.107934
» http://doi.org/10.1016/j.jobe.2023.107934 -
30 J. M. Franco de Carvalho, W. C. Fontes, C. F. de Azevedo, G. J. Brigolini, W. Schmidt, and R. A. F. Peixoto, "Enhancing the eco-efficiency of concrete using engineered recycled mineral admixtures and recycled aggregates," J. Clean. Prod., vol. 257, pp. 120530, 2020, http://doi.org/10.1016/j.jclepro.2020.120530
» http://doi.org/10.1016/j.jclepro.2020.120530 -
31 K. Robalo, E. Soldado, H. Costa, L. Carvalho, R. do Carmo, and E. Júlio, "Durability and time-dependent properties of low-cement concrete," Materials (Basel), vol. 13, no. 16, pp. 3583, 2020, http://doi.org/10.3390/ma13163583
» http://doi.org/10.3390/ma13163583 -
32 A. E. Klausen, T. Kanstad, Ø. Bjøntegaard, and E. Sellevold, "Comparison of tensile and compressive creep of fly ash concretes in the hardening phase," Cement Concr. Res., vol. 95, pp. 188–194, 2017, http://doi.org/10.1016/j.cemconres.2017.02.018
» http://doi.org/10.1016/j.cemconres.2017.02.018 -
33 S. H. Chu, "Effect of paste volume on fresh and hardened properties of concrete," Constr. Build. Mater., vol. 218, pp. 284–294, 2019, http://doi.org/10.1016/j.conbuildmat.2019.05.131
» http://doi.org/10.1016/j.conbuildmat.2019.05.131 -
34 A. C. P. Martins, J. M. Franco de Carvalho, M. N. Duarte, L. G. Pedroti, J. C. L. Ribeiro, and R. A. F. Peixoto,"Use of steel slag and LAS-based modifying admixture in obtaining highly eco-efficient precast concrete products," J. Build. Eng., vol. 66, pp. 105884, 2023, http://doi.org/10.1016/j.jobe.2023.105884
» http://doi.org/10.1016/j.jobe.2023.105884 -
35 J. M. Franco de Carvalho, W. Schmidt, H.-C. Kühne, and R. A. F. Peixoto, "Influence of high-charge and low-charge PCE-based superplasticizers on Portland cement pastes containing particle-size designed recycled mineral admixtures," J. Build. Eng., vol. 32, pp. 101515, 2020, http://doi.org/10.1016/j.jobe.2020.101515
» http://doi.org/10.1016/j.jobe.2020.101515 -
36 D. P. Bentz, A. S. Hansen, and J. M. Guynn, "Optimization of cement and fly ash particle sizes to produce sustainable concretes," Cement Concr. Compos., vol. 33, no. 8, pp. 824–831, 2011, http://doi.org/10.1016/j.cemconcomp.2011.04.008
» http://doi.org/10.1016/j.cemconcomp.2011.04.008 - 37 P. K. Mehta, and P. Monteiro, Concrete: Microstructure, Properties, and Materials, 4th ed., New York, McGraw Hill, 2014.
- 38 P. K. Mehta, "High-performance, high-volume fly ash concrete for sustainable development," in: Proc. Int. Workshop on Sustainable Development and Concrete Technology, 2004, pp. 3–14.
- 39 Associação Brasileira de Normas Técnica, Portland Cement - Requirements, NBR 16697, 2018.
-
40 D. R. Gonçalves, W. C. Fontes, J. C. Mendes, G. J. Silva, and R. A. Peixoto, "Evaluation of the economic feasibility of a processing plant for steelmaking slag," Waste Manag. Res., vol. 34, no. 2, pp. 107–112, 2016, http://doi.org/10.1177/0734242X15615955
» http://doi.org/10.1177/0734242X15615955 -
41 J. N. Sant’ana Filho, S. N. Da Silva, G. C. Silva, J. C. Mendes, and R. A. F. Peixoto, "Technical and environmental feasibility of interlocking concrete pavers with iron ore tailings from tailings dams," J. Mater. Civ. Eng., vol. 29, no. 9, 2017. http://doi.org/10.1061/(ASCE)MT.1943-5533.0001937
» http://doi.org/10.1061/(ASCE)MT.1943-5533.0001937 -
42 H. D. Andrade, J. M. F. de Carvalho, L. C. B. Costa, F. P. F. Elói, K. D. C. e Silva, and R. A. F. Peixoto, "Mechanical performance and resistance to carbonation of steel slag reinforced concrete," Constr. Build. Mater., vol. 298, pp. 123910, 2021, http://doi.org/10.1016/j.conbuildmat.2021.123910
» http://doi.org/10.1016/j.conbuildmat.2021.123910 -
43 L. C. B. Costa, M. A. Nogueira, L. C. Ferreira, F. P. F. Elói, J. M. F. de Carvalho and R. A. F. Peixoto, "Eco-efficient steel slag concretes: an alternative to achieve circular economy," Rev. IBRACON Estrut. Mater. vol. 15, no. 2, pp. e15201, 2022. https://doi.org/10.1590/s1983-41952022000200001
» https://doi.org/10.1590/s1983-41952022000200001 - 44 Associação Brasileira de Normas Técnica, Hardened mortar and concrete - Determination of absorption. voids and specific gravity, NBR 9778, 2005.
- 45 ASTM International, Standard Test Method for Density, Absorption, and Voids in Hardened Concrete, C642, 2021.
- 46 Associação Brasileira de Normas Técnica, Hardened concrete — Determination of ultrasonic wave transmission velocity, NBR 8802, 2013.
-
47 ASTM International, Standard Test Method for Pulse Velocity Through Concrete, C597, 2016. http://doi.org/10.1520/C0597-16
» http://doi.org/10.1520/C0597-16 - 48 ASTM International, Standard test method for fundamental transverse, longitudinal, and torsional frequencies of concrete specimens, C215, 2014.
- 49 Associação Brasileira de Normas Técnica, Concrete - Compression test of cylindrical specimens, NBR 5739, 2018.
- 50 ASTM International, Standard Test Method for Compressive Strength of Cylindrical Concrete Specimens, C39, 2018.
- 51 Associação Brasileira de Normas Técnica, Concrete and mortar - Determination of the tensile strength by diametrical compression of cylindrical specimens, NBR 7222, 2011.
- 52 ASTM International, Tensile Testing for Concrete Surfaces, C1583, 2010.
- 53 J.C. Mendes, Thermal Properties of Cement-based Composites, Tese de doutorado, PROPEC, Univ. Fed. Ouro Preto, Ouro Preto, 2019.
- 54 Associação Brasileira de Normas Técnica, Design of reinforced concrete structures – Procedure, NBR 6118, 2014.
- 55 Associação Brasileira de Normas Técnica, Hardened concrete - Determination of the volumetric electric resistivity, NBR 9204, 2004.
- 56 ASTM International, Standard Test Method for Bulk Electrical Resistivity or Bulk Conductivity of Concrete, C1876, 2019.
- 57 Associação Brasileira de Normas Técnica, Housing buildings - Performance, NBR 15575, 2013.
-
58 H. D. Andrade, J. M. F. de Carvalho, L. C. B. Costa, F. P. da Fonseca Elói, K. D. do Carmo e Silva and R. A. F. Peixoto, "Mechanical performance and resistance to carbonation of steel slag reinforced concrete," Constr. Build. Mater., vol. 298, pp. 123910, 2021, http://doi.org/10.1016/j.conbuildmat.2021.123910
» http://doi.org/10.1016/j.conbuildmat.2021.123910 -
59 S. Bishnoi, RILEM Bookseries Calcined Clays for Sustainable Concrete, in: Proc. 3rd Int. Conf. Calcined Clays for Sustainable Concrete, 2022, http://www.springer.com/series/8781 (accessed Sep. 30, 2024).
» http://www.springer.com/series/8781 - 60 G. Pessôa, J. D. C. Dominguéz, and J. S. de Carvalho, "Porosidade do concreto determinada por microtomografia com raios X e processamento de imagem," Eng. Estud. Pesqui., vol. 14, pp. 20–26, 2014.
- 61 G. Pessôa, "Porosidade do concreto determinada por microtomografia com raios X e processamento de imagem," Eng. Estudo Pesqui., vol. 14, pp. 20–26, 2014.
-
62 V. R. Carvalho, L. C. B. Costa, F. P. F. Elói, A. C. S. Bezerra, J. M. F. Carvalho, and R. A. F. Peixoto, "Performance of low-energy steel slag powders as supplementary cementitious materials," Constr. Build. Mater., vol. 392, pp. 131888, 2023, http://doi.org/10.1016/j.conbuildmat.2023.131888
» http://doi.org/10.1016/j.conbuildmat.2023.131888 -
63 F. Saint-Pierre, A. Philibert, B. Giroux, and P. Rivard, "Concrete quality designation based on ultrasonic pulse velocity," Constr. Build. Mater., vol. 125, pp. 1022–1027, 2016, http://doi.org/10.1016/j.conbuildmat.2016.08.158
» http://doi.org/10.1016/j.conbuildmat.2016.08.158 - 64 R. B. C. Sales, "Estudo de compostos de cimento Portland utilizando o ensaio de frequência ressonante forçada e termografia," Tese de doutorado, Univ. Fed. Minas Gerais, Belo Horizonte, 2008.
- 65 M. B. Santos and J. De Brito, Susceptibilidade dos agregados reciclados no desenvolvimento da reacção álcalis-sílica: o que pode mudar?. Revista de Engenharia Civil, no. 55, pp. 36–46, 2018. Accessed Sep. 30, 2024. [Online]. Available: http://www.civil.uminho.pt/revista
- 66 A.G. Gumieri, "Study of the technical viability in the use of bof slags as a Mineral admixture in cement," Tese de doutorado, Univ. Fed. Rio Gde. Sul, Porto Alegre, 2002.
-
67 S. Z. Carvalho, F. Vernilli, B. Almeida, M. Demarco, and S. N. Silva, "The recycling effect of BOF slag in the portland cement properties," Resour. Conserv. Recycling, vol. 127, pp. 216–220, 2017, http://doi.org/10.1016/j.resconrec.2017.08.021
» http://doi.org/10.1016/j.resconrec.2017.08.021 -
68 N. H. Roslan, M. Ismail, Z. Abdul-Majid, S. Ghoreishiamiri, and B. Muhammad, "Performance of steel slag and steel sludge in concrete," Constr. Build. Mater., vol. 104, pp. 16–24, 2016, http://doi.org/10.1016/j.conbuildmat.2015.12.008
» http://doi.org/10.1016/j.conbuildmat.2015.12.008 -
69 Q. Wang, J. Yang, and P. Yan, "Cementitious properties of super-fine steel slag," Powder Technol., vol. 245, pp. 35–39, 2013, http://doi.org/10.1016/j.powtec.2013.04.016
» http://doi.org/10.1016/j.powtec.2013.04.016 -
70 A. Santamaría, A. Orbe, J. T. S. José, and J. J. González, "A study on the durability of structural concrete incorporating electric steelmaking slags," Constr. Build. Mater., vol. 161, pp. 94–111, 2018, http://doi.org/10.1016/j.conbuildmat.2017.11.121
» http://doi.org/10.1016/j.conbuildmat.2017.11.121 -
71 Y. Biskri, D. Achoura, N. Chelghoum, and M. Mouret, "Mechanical and durability characteristics of High Performance Concrete containing steel slag and crystalized slag as aggregates," Constr. Build. Mater., vol. 150, pp. 167–178, 2017, http://doi.org/10.1016/j.conbuildmat.2017.05.083
» http://doi.org/10.1016/j.conbuildmat.2017.05.083 - 72 American Association of State Highway and Transportation Officials, Standard Method of Test for Electrical Resistivity of a Concrete Cylinder Tested in a Uniaxial Resistance Test, TP 119, 2015.
- 73 ASTM, Standard Test Method for Electrical Indication of Concrete’s Ability to Resist Chloride Ion Penetration, C1202 – 12, 2012.
-
74 B. L. Damineli, F. M. Kemeid, P. S. Aguiar, and V. M. John, "Measuring the eco-efficiency of cement use," Cement Concr. Compos., vol. 32, no. 8, pp. 555–562, 2010, http://doi.org/10.1016/j.cemconcomp.2010.07.009
» http://doi.org/10.1016/j.cemconcomp.2010.07.009