ABSTRACT
The global warming and carbon footprints of cement production has increased the demand for sustainable binders. One-part geopolymer concrete(OGPC) has emerged as a promising alternative offering simplified handling similar to OPC. Despite the growing researches, limited studies focused on solid activators for ambient-cured OGPC. This study investigates the influence of hybrid solid activator systems comprising sodium hydroxide (NaOH), sodium metasilicate (Na2SiO3) and sodium carbonate (Na2CO3) in different combinations on ambient-cured OGPC based on Fly Ash and GGBS. Fresh and hardened concrete performance of these mixes were correlated with microstructural analysis through SEM-EDS and XRD. Hybrid activation using NaOH-Na2SiO3 enhanced the reaction kinetics resulting in a denser matrix, characterised by the co-existence of N-A-S-H and C-A-S-H gels and achieved 28-day compressive strength of approximately 39 MPa, about 37% higher than OPC. The Na2SiO3 system demonstrated about 17% higher strength than OPC, whereas Na2CO3 system exhibited poor performance due to lower alkalinity. Durability and material cost analysis further revealed that hybrid NaOH-Na2SiO3 system offered most economical performance among the mixes studied. The findings highlight the relationship between the microstructure, mechanical performance and durability in OGPC, emphasizing the critical role of solid activators in governing dissolution behaviour, gel formation and mechanical performance in ambient-cured OGPC.
Keywords:
One-part geopolymer concrete; Hybrid solid activators; Ambient cured-geopolymer; Fly ash; Ground granulated blast furnace slag; Geopolymerization.
1. INTRODUCTION
Rising global warming and increasing carbon dioxide (CO2) emissions pose serious challenges to the construction industry with cement production being a significant contributor. In 2022, the cement industry alone generated approximately 1.6 billion metric tonnes of CO2, and around 332 kg CO2 is emitted for casting each cubic meter of conventional concrete [1]. Although this imposes an environmental cost, cement cannot be replaced in infrastructure construction, driving research towards low carbon alternatives such as geopolymer concrete (GPC). Geopolymer concrete utilizes industrial by-products such as fly ash and ground granulated blast furnace slag (GGBS), thereby promoting waste recycling and circular economy principles. Previous studies reported that GPC can reduce environmental impact by 50-60% and consumes significantly less energy and emits lower CO2 compared to ordinary Portland cement (OPC) [2,3,4]. The extensive use of GPC is however restricted by practical issues concerning traditional two-part systems where highly aggressive alkaline liquid activators including sodium hydroxide and sodium metasilicate are utilized. These liquid activators are difficult to handle and require skilled labour, limiting the field applicability of two-part GPC in in-situ construction in countries like India, where availability of skilled labour is limited [5, 6]. To overcome these limitations, one-part geopolymer concrete (OGPC) was developed, as a safer and more practical alternative. In OGPC, solid activators are premixed with aluminosilicate precursors and water is added at the site thus, the “just-add-water” concept arrived. According to the life cycle assessments, OGPC has less environmental impact up to 24% than OPC and 23% than two-part GPC because it uses no energy intensive liquid activators [3], [4]. OGPC attains strength by the process of geopolymerization similar to two-part systems, where the dissolution of aluminosilicate material in alkaline solution followed by polycondensation occurs to create a rigid binding gel [7]. GPC is much more resistant to chemical attack, carbonation, freeze and thaw and high temperature exposure than OPC [8, 9].
Recent studies have demonstrated that the performance of one-part geopolymer systems strongly depends on activator chemistry, calcium availability, curing regime and precursor reactivity, particularly under ambient curing conditions where slower geopolymerization kinetics often limits early strength development [10,11,12,13]. Despite its effectiveness, sodium metasilicate based activation is associated with higher economic and environmental cost, limiting large-scale practical implementation [10]. A safer and more sustainable alternative that has been recommended is sodium carbonate, which has lower alkalinity and thus causes slow reaction kinetics and low early strength [14]. A comparative literature based assessment of OPC, two-part geopolymer concrete and one-part geopolymer systems reported in recent studies is presented in Table 1.
The CO2 reduction of geopolymer concrete has been reported recently to be about 30–70% less than that of OPC concrete based on the composition of precursors, type of activator used and curing conditions [15]. However, the mechanical properties of conventional two-part geopolymer systems are quite good, while the handling and safety issues due to the use of liquid alkaline activators are the major problems. The one-part geopolymer concrete is a more viable solution for the field application with lower environmental impact.
Previous research on OGPC has mostly focused on the systems with sodium metasilicate or sodium carbonate as the activator or the systems with sodium metasilicate and sodium carbonate in small proportions [16]. Use of NaOH in OGPC systems will fasten the dissolution of Si-Al species in precursor enhancing the quick setting of matrix, especially under ambient curing. This makes the OGPC more similar to conventional OPC. On the other hand, activation and strength development through the addition of solid sodium hydroxide pellets, especially when used along with sodium metasilicate and sodium carbonate, has not been well studied, even though two-part GPC systems have shown improved activation and strength development with sodium hydroxide [19]. Thus, there is a significant research gap concerning the systematic assessment of a hybrid solid activator system of sodium hydroxide, sodium metasilicate and sodium carbonate in OGPC, particularly when the specimens are cured at ambient room temperature. The performance of OGPC with hybrid solid activator systems for practical ambient curing and their influence on the reaction kinetics and the relationship between microstructural property and strength performance is underexplored. Also, to enable faster hardening of OGPC mixes, GGBS was intentionally provided in higher proportions in all the mixes. The higher calcium content in GGBS helps to form C-A-S-H gel in addition to N-A-S-H gel, leading to denser and high strength matrix [20]. The novelty of this study lies in the systematic evaluation of hybrid solid activator blends for ambient cured one-part geopolymer concrete and in establishing the relationship between activator chemistry, reaction products, microstructural characteristics and mechanical performance.
Based on the above discussion, this study investigates the influence of sodium hydroxide, sodium metasilicate and sodium carbonate based solid activator system on the fresh and mechanical properties of fly ash and GGBS based one-part geopolymer concrete cured under ambient room temperature. The study also examines the microstructure and morphology of the developed geopolymer systems through scanning electron microscopy and X-ray diffraction to study the relationships between the products of the reaction and the strength formation. It is hypothesized that hybrid solid activator systems with optimized alkalinity and silica availability can enhance geopolymerization under ambient curing, resulting in improved matrix continuity and mechanical performance. Thus, this work attempts to establish an effective and feasible hybrid solid activator system that will be applicable in ambient cured one-part geopolymer concrete with potential usage in sustainable construction. The present study is limited to ambient curing conditions and short-term mechanical performance up to 28 days.
2. MATERIALS AND METHODS
2.1. Materials used
Low-calcium Class F fly ash (FA), obtained as a by-product from thermal power plants was used as the primary aluminosilicate precursor in this study. Fly ash is considered for its high silica content. Fly ash particles are finer than ordinary Portland cement which contributes to the formation of a denser matrix with reduced pore structure [21, 22]. The physical properties and chemical composition of fly ash are presented in Tables 2 and 3 respectively. The Si/Al ratio of fly ash used in this study was 1.6 which is favourable for geopolymerization as it promotes the formation of stable aluminosilicate gel networks contributing to improved matrix stability and mechanical performance [13].
Ground granulated blast furnace slag (GGBS), a by-product of the steel industry was used as a secondary precursor material. Table 3 illustrates that GGBS contains high levels of calcium oxide (CaO). The high CaO content promotes the formation of C-A-S-H gel, which accelerates the geopolymerization reaction resulting in a denser matrix and reduced setting time. Therefore, GGBS based systems exhibited comparatively higher early strength development. GGBS also allows the systems to be cured at ambient room temperature avoiding heat curing, which is otherwise necessary in the low calcium fly ash based geopolymer systems [23]. Therefore, GGBS was incorporated in relatively higher proportions to increase calcium availability, accelerate ambient temperature geopolymerization and promote the formation of additional C-A-S-H gel responsible for early strength development. Both GGBS and FA are brought in ultrafine powder form from the supplier [24].
Three types of solid alkaline activators were used in this study, namely sodium hydroxide pellets, sodium metasilicate and anhydrous sodium carbonate. Commercial grade Sodium hydroxide pellets with approximately 98% purity and anhydrous sodium carbonate with approximately 99% purity were used. Sodium metasilicate is used in pentahydrate form (Na2SiO3.5H2O) of laboratory grade with minimum Na2O content of 28% was used in the study. The silicate modulus of sodium metasilicate was close to 1.0 with Na2O:SiO2 ratio as approximately 1:1, indicating nearly equal proportion of SiO2 and Na2O. Sodium hydroxide exhibits a pH value of approximately 12 when dissolved in 5% water, while sodium metasilicate and anhydrous sodium carbonate exhibit pH values of approximately 11.5 (10% solution) and 11.0 (5% solution), respectively. These activators were used in different combinations, as detailed in Table 4. Sodium metasilicate provides additional soluble silica, enhancing polymerization and gel formation [25]. Sodium hydroxide with theoretical Na2Oeq of around 0.775 provides the alkali environment that is necessary for the dissolution of silica and alumina in the precursor [26]. Even though sodium hydroxide is widely used in two-part geopolymers, it is not widely used in one-part systems. Sodium carbonate having low Na2Oeq of about 0.58 is considered safer and more environmentally friendly and less expensive compared to sodium hydroxide. However, its lower alkalinity results in slower reaction kinetics thus, achieving comparable mechanical performance generally requires longer curing durations. This behaviour is because of the carbonate ions interfering with dissolved calcium species, thereby hindering the formation of C-A-S-H and N-A-S-H gel [14]. The selection of hybrid activator systems was intended to balance alkalinity, silica availability, reaction kinetics and practical handling characteristics under ambient curing conditions. All the activators were used in as received condition without any further treatment.
The coarse aggregates used in this study consisted of well-graded, crushed angular aggregates with a nominal maximum size of 20 mm, free from clay and deleterious materials. Manufactured sand (M-sand) conforming to Zone II grading was used as fine aggregate [27]. Aggregate grading is very important in gaining efficient void filling and enhanced packing density [28]. The aggregates employed in geopolymer concrete were also chosen in accordance with IS 383:2016 same as that of ordinary Portland cement concrete [29, 30]. Poorly graded aggregates may reduce packing density resulting in less cohesive mix and reduced mechanical strength. Figure 1 gives the overall summary of the work carried out in this study.
2.2. Experimental methods
The Fresh and hardened property tests were conducted on geopolymer concrete (GPC) to evaluate workability, setting characteristics and mechanical performance. Workability refers to the ease with which concrete can be mixed, placed and compacted without segregation or bleeding and is influenced by factors such as alkaline activator concentration, silicate modulus, precursor fineness and curing regime. In the present study, the slump cone test for all mixes resulted in zero slump, as GPC is typically high cohesive and exhibits low slump. Thus, a flow table test in accordance with IS 1199 (part6) 2018 was used as reliable test to determine the workability of these stiff geopolymer mixes.
The Vicat apparatus was used to determine the setting characteristics of OGPC in accordance with IS 4031 (Part 5): 1988 which are primarily influenced by precursor reactivity, activator dissolution and reaction kinetics. The setting characteristics were evaluated to study the influence of activator dissolution and precursor reactivity on early geopolymerization behaviour. The compressive strength was conducted on 150 mm × 150 mm × 150 mm cube specimens at 7, 14 and 28 days with a 200-ton universal testing machine at the loading rate of 2 kN/s in accordance with IS 516:1999 and compared with the results of OPC and two-part geopolymer concrete [31]. Split tensile strength tests as per IS 5816:1999 were used to determine tensile behaviour on cylindrical specimens with 150 × 300 mm dimensions. The specimens were loaded at a steady rate of 1 kN/min till splitting failure was found, which gives an insight into cracking resistance and tensile performance [32]. The flexural strength was assessed in prism specimens of size 100 mm × 100 mm × 300 mm by three-point bending as per IS 516 :1959. The failure of the specimen at the tensile face side was used to assess the flexural performance of the concrete. For each mix and testing age, three specimens were tested and the average value was reported in the study [31].
The correlation between morphology, phase composition and mechanical performance of one-part geopolymer concrete was established through microstructural and phase analyses for 28-day specimen of one-part geopolymer concrete [33]. Scanning Electron Microscope Analysis was conducted with Carl Zeiss Sigma 300 microscope model equipped with Smart EDX-Energy Dispersion System. The microscope operated at an acceleration voltage ranging from 0.02 kV to 30 kV with a resolution of 1.0 nm at 15 kV and 1.6 nm at 1 kV. Phase composition analysis was carried out using Bruker D8 Advance diffractometer. SEM analysis was conducted to examine the surface morphology, gel formation and pore distribution in order to evaluate the extent of geopolymerization, matrix densification [34]. The XRD analysis was designed to determine the crystalline and amorphous phases of the binder matrix to complement the findings of SEM. Durability and cost analysis of the mixes were carried out to study the long-term serviceability and economic feasibility of the OGPC mixes.
2.3. Mix proportion
The mix proportions of the various geopolymer concrete samples are presented in Table 4. For SH, SS mixes, the activator to binder ratio was maintained at 0.10, corresponding to 10% of the binder weight while, for SC mix activator to binder ration was 0.125. This activator to binder ratio of 0.10 and 0.125 was selected based on the previous literatures and preliminary optimization to ensure sufficient activator dissolution, controlled alkalinity and stable setting behaviour under ambient curing conditions. The sodium metasilicate to sodium hydroxide ratio was fixed at 2.0, while the sodium metasilicate to sodium carbonate ratio was maintained at 2.5 [35]. These proportion were selected to maintain suitable silica availability and alkalinity necessary for polycondensation to form denser matrix. The water to binder ratio was maintained at 0.35, which is equivalent to M30 grade concrete [24].
All mix proportions are expressed in kilograms per cubic meter (kg/m3) of concrete unless otherwise stated. In all the mixes the fly ash was added to 30% and the GGBS for 70% of the total precursor composition except in SS1 mix where GGBS was added to 80% and it was shown in Table 5. TGPC mix is the two-part GPC concrete and was proportioned independently using liquid activators. The TGPC sample contains the same precursor proportions and liquid activator (NaOH- 61.33 litres and Na2SiO3 -122.67 litres). Standard OPC of M30 grade without any admixtures was used as benchmark for testing GPC sample performances. The higher proportion of GGBS was intentionally adopted to enhance calcium availability for C-A-S-H gel formation. The water to binder ratio of 0.35 was used to ensure sufficient workability and activator concentration [12]. The selected activator combinations were designed to investigate the influence of varying alkalinity and soluble silica availability on geopolymerization behaviour and mechanical performance under ambient curing condition. The mix designation SH represent sodium hydroxide-sodium metasilicate activation, SS represents sodium metasilicate activation and SC represents sodium silicate-sodium carbonate activation.
2.4. Specimen fabrication and curing
The mixing procedure and duration significantly influence the workability and homogeneity of geopolymer concrete. Adequate mixing time was essential to ensure uniform dispersion and dissolution of solid activators, thereby increasing mix homogeneity and polymerization efficiency [10]. Machine mixing was adopted to ensure better workability and uniformity, as hand mixing produces lean and stiff mixes, that were difficult to handle. The increased dissolution of solid activators makes this possible, as better blending leads to uniform dissolution and helps in a uniform geopolymerization. Initially, the dry materials including M-sand, coarse aggregates, FA, GGBS and the solid activators were sequentially mixed thoroughly to ensure homogeneity of solid activators before the addition of water. Calculated quantity of water was then added gradually in portions and the mixture was continuously mixed for approximately 5 minutes to achieve uniform and cohesive mix. The concrete was then poured into standard moulds in three layers in agreement with the corresponding tests and compacted with the help of a table vibrator. Vibration was applied for 5 seconds per layer to eliminate entrapped air, beyond which segregation was observed. The compacting process was shown in Figure 2. The specimens were demoulded after 24 hours of casting. Only the carbonate activated system requires more setting time hence those were demoulded after 48 hours.
Conventionally, geopolymer concrete requires heat curing at temperatures ranging from 60°C to 90°C for durations of 6 to 24 hours to achieve adequate strength development [36]. However, these methods are not feasible for in-situ concrete works. Therefore, ambient curing was adopted to simulate practical field conditions and evaluate the feasibility of hybrid solid activator systems without external thermal energy input. The ambient curing under the in-situ room temperatures of about 20 °C to 30 °C was implemented in this study to make the curing more similar to OPC. Even though strength development in ambient cured geopolymer is relatively slower than that of heat cured geopolymer, because of slower reaction kinetics, it results in stable and more durable microstructural development with time [31]. Maintaining a constant ambient temperature facilitates gradual polymerisation and contributes to the formation of a dense and durable matrix with improved long-term performance [32]. Also, eliminating the need for external heating significantly reduces CO2 emissions associated with the curing process [31].
Ambient room temperature curing was done by wrapping the specimens in plastic sheets and kept in laboratory temperature of 27 ± 2ºC and relative humidity of approximately 60–70% and this is shown in Figure 3. The wrapping helps prevent the moisture loss during the initial curing stage. Although, the early age strength development was comparatively slower under ambient curing, considerable strength gain was observed at later curing ages. The curing of the specimens was done for 7, 14 and 28 days until which the wrapping was maintained. Also keeping these SC specimens unwrapped produced efflorescence due to reaction with atmosphere.
3. RESULTS AND DISCUSSION
3.1. Setting time
The setting characteristics of geopolymer concrete were evaluated using the paste extracted from the corresponding geopolymer concrete mix prepared. The Vicat test shown in Figure 4 was used to evaluate the early stiffening behaviour of GPC systems, where the initial setting time corresponds to the loss of workability due to the early gel formation and final setting time corresponds to the development of rigid aluminosilicate network. The result given in Table 6 showed that the mixes containing sodium hydroxide exhibited relatively shorter setting time compared to other systems. The initial setting time of the SH standard is few minutes less than the standard initial setting (not less than 30 minutes) of conventional concrete [37]. The shorter setting time observed in NaOH activated systems can be attributed to higher alkalinity of NaOH, which accelerates the dissolution of aluminosilicate species and promotes rapid gel formation. In contrast, the sodium metasilicate activated systems exhibited relatively delayed setting due to relatively low alkalinity leading to slower dissolution kinetics and gradual gel formation. The comparatively extended setting time of sodium metasilicate activated systems may provide improved workability and handling during practical field applications. The sodium carbonate activated system exhibited longest setting time. SC mix exceeded the standard final setting time (not more than 600 minutes) due to its low alkalinity and slower dissolution of aluminosilicate species. In addition, carbonate ions tend to retard geopolymerization by limiting the rapid formation of C-A-S-H and N-A-S-H gels, resulting in delayed hardening behaviour. Consequently, SC specimens required extended curing duration to achieve sufficient hardening under ambient conditions. Overall, one-part geopolymer systems showed relatively slower setting behaviour than two-part system because the solid activators require prior dissolution in the water before initiating dissolution of Si and Al species and geopolymerization reaction. Similar trends in setting behaviour have been reported in previous studies on ambient cured one-part geopolymer systems, where activator alkalinity and calcium availability significantly influenced reaction kinetics and hardening characteristics [21, 23].
3.2. Flow test
Workability of geopolymer mixes were evaluated using flow table test, in terms of average flow diameter measured in two perpendicular directions and is presented in Table 7. The slump of the SH was presented in Figure 5 which illustrates the quick setting of SH mix. The sodium metasilicate activated system exhibited relatively higher flow compared to sodium hydroxide system and it was given in Figure 6. The lower flowability observed in NaOH activated system can be attributed to the rapid dissolution of aluminosilicate species and quick gel formation, which increased viscosity of the mix and reduced the flowability. Whereas, sodium metasilicate based system exhibited comparatively improved flowability due to slower reaction kinetics and enhanced cohesiveness of the paste, which delayed premature stiffening during mixing. All mixes especially SH mix achieved nearly zero slump because of the highly cohesive nature of geopolymer systems. However, these mixes achieved flow percentage in the range of 100–110% which falls under medium workability range for conventional placement and vibratory compaction methods as per the standards [38]. The alkalinity of the activators, the soluble silica content and the rate of gel formation of these mixes have a significant effect on their flow behaviour, which in turn influences the rheological properties and viscosity of the fresh mix [39].
The flowability of the geopolymer mixes can be further improved by adding admixtures without increasing the water to binder ratio, as higher water content may dilute the activator concentration and negatively influence the geopolymerization and mechanical performance.
3.3. Evaluation of mechanical performance of GPC
3.3.1. Compressive strength test
The compressive strength development of GPC varied significantly with the type of alkaline activator as shown in Table 8 and Figure 7. Among all mixes, the sodium hydroxide (SH) activated system exhibited the highest strength gain, reaching 38.98 MPa (N/mm2) at 28 days which was approximately 37% higher than OPC under similar curing condition. This is comparable to that reported for two-part geopolymer concrete systems cured under similar conditions and is significantly higher than that of OPC. The failure of the samples was illustrated in Figure 8. Previous studies on one-part geopolymer concrete activated using sodium silicate and hydroxide systems under ambient curing have reported lower 28 day compressive strengths, typically in the range of 35 to 37 MPa, particularly when lower GGBS contents were used [10]. The superior performance of SH mix can be attributed to the higher alkalinity of NaOH which accelerated the dissolution of aluminosilicate species and forming larger SiO and AlO monomers. These monomers polycondensed into a continuous geopolymertic network while, the calcium from GGBS promoted the simultaneous formation of C-A-S-H gel in addition to N-A-S-H gel, resulting in reduced porosity and increased matrix continuity, responsible for higher compressive strength development, which is similar to the trends seen in previous studies [33].
The sodium silicate activated mix (SS) showed relatively moderate performance, with a considerable strength increase of 33.54 MPa after 28 days representing effective polymerisation and gradual development of aluminosilicate gel network under ambient curing condition. On the other hand, the SS2 mix, with an increased amount of fly ash had lower strength (25.81 MPa at 28 days), which can be attributed to slower reaction kinetics associated with increased fly ash content and comparatively lower calcium content. This is the reason for reduced early gel formation and delayed matrix densification. In FA and GGBS binder system, the presence of calcium contributed to the co-existence of C-A-S-H and N-A-S-H gels leading to the formation of denser matrix, reduced pore structure and enhanced compressive strength, which was further confirmed through the microstructural observation done in SEM and XRD Analysis [33]. On the other hand, the sodium carbonate (SC) system demonstrated the least performance (15.24 MPa at 28 days), which may be attributed to its weaker alkalinity leading to limited dissolution of aluminosilicate precursors and slower geopolymerization kinetics. The slower reaction kinetics is due to the carbonate ions hindering the formation of continuous Al-Si network in the polymerization process which increased the availability of connected pores. Thus SC system forms less dense matrix leading to poor compressive strength performance. Improved performance of sodium carbonate activated systems in the previous studies were achieved through elevated temperature curing, which can accelerate precursor dissolution and geopolymerization reactions [14].
Overall, the results demonstrate that the activator chemistry and curing duration play crucial roles in governing geopolymerization behaviour and strength development in ambient cured OGPC systems. The most effective mechanical performance was produced by the hybrid sodium hydroxide-sodium metasilicate activation, due to enhanced reaction kinetics and gel formation, whereas sodium carbonate activation exhibited slower strength development because of reduced alkalinity and delayed geopolymerization. Similar trends have been reported in previous studies on ambient cured geopolymer systems, where increased activator alkalinity and calcium availability significantly improved strength development and the sodium availability for charge balancing the aluminosilicate network improved microstructure [21, 23, 25].
3.3.2. Split tensile strength test
The split tensile strength results showed a similar trend with compressive strength development. The test results were given in Table 9 and Figure 9. The SH mix exhibited the highest performance, indicating strong binder cohesion, improved interfacial bonding and formation of a more continuous polymeric network. The obtained tensile strength was comparable to two-part GPC system and higher than conventional OPC under similar curing conditions. Previous studies involving lower GGBS contents reported comparatively lower tensile strength development with similar activator systems. The more continuous and interconnected aluminosilicate gel network formed due to the hybrid action of sodium hydroxide and sodium silicate, resulting in stronger particle bonding and improved resistance to crack initiation under indirect tensile loading. Similar observations have been reported in previous studies, where hybrid alkaline activators enhanced matrix continuity and tensile performance under ambient curing conditions. SS1 mix displayed moderate performance, suggesting that soluble silica contributed to gradual formation of aluminosilicate gel network although its contribution to tensile resistance was less compared to its compressive strength.
SS2 mix exhibited gradual strength development, however, its tensile strength remained lower than SS1. The higher fly ash content in SS1 mix reduced the overall calcium availability within the binder system. Since the FA reacts slower than GGBS under ambient condition the development of a continuous binding matrix was delayed, leading to reduced tensile strength. These results indicate that, under ambient curing, an appropriate balance between reactive calcium and soluble silica is important for improving crack resistance and tensile behaviour.
The sodium carbonate (SC) system exhibited the lowest strength, which can be attributed to its limited dissolution capacity and weaker bond formation resulting from the lower alkalinity of sodium carbonate activation. carbonate ions can temporarily consume available calcium through the formation of carbonate-containing phases, delaying the development of calcium-rich reaction products. Consequently, the binder matrix remained relatively porous with weaker particle bonding, making the material more susceptible to crack initiation and propagation under tensile loading.
The tensile performance of One-part GPC in comparison with control mixes are given in Table 9 and its trend is shown in Figure 9. These results highlighted the enhanced gel formation and improved particle bonding in the SH and SS mixes. Figure 10 illustrates the crack propagation under split tensile test. Hence, in FA and GGBS system, the presence of sodium helps in the formation denser matrix and the occurrence of calcium helps in development of additional C-A-S-H network resulting in reduces micro crack initiation under tensile loading [23, 25]. The improved tensile performance observed in SH and SS systems was consistent with SEM observations showing a denser matrix and reduced pore structure.
3.3.3. Flexural strength test
The flexural strength test results presented in Table 10 and Figure 11 indicate that SH mix consistently achieved the highest flexural strength due to accelerated dissolution of aluminosilicate precursors by sodium hydroxide along with the additional soluble silica supplied by sodium metasilicate. This promotes extensive polycondensation reaction forming dense aluminosilicate binder matrix also, the calcium from GGBS helps in the formation of more refined matrix with strong interfacial bonding between the aggregates. Although the flexural strength of SH mix was slightly lower than two-part GPC system and OPC due the presence of unreacted FA in the binder system.
The SS1 and SS2 mixes achieved moderate strength due the absence of NaOH to enhance the polycondensation and the high FA content in SS1 diminishing the calcium supply by GGBS delaying early densification of the matrix. This results in less effective matrix refinement and lower resistance to crack propagation. These observations suggest that the balance between calcium availability and activator alkalinity is an important factor for achieving high flexural performance. The comparatively lowest flexural strength of the SC mix further indicates incomplete matrix densification under ambient curing conditions due to delayed geopolymerization kinetics. Thus, the hardened matrix had a less continuous binder phase and less interparticle bonding, which were more susceptible to crack growth under bending stresses. Similar trends of flexural strength have been reported in carbonate-activated geopolymer systems under ambient curing [21, 23].
Overall, the hybrid sodium hydroxide-sodium metasilicate activation provided superior flexural performance due to enhanced reaction kinetics and network connectivity, while silicate based systems showed promising improvements in the long run. Carbonate-based activators exhibited inferior performance for ambient cured condition.
At 28 days, the SH mix achieved approximately 62% higher flexural strength than the SS system and exhibited performance comparable to two-part geopolymer concrete. Similar flexural strength trends have been reported in ambient cured geopolymer systems where higher alkalinity. The flexural strength trends were consistent with the microstructural observations obtained from SEM and XRD analyses, which confirmed improved gel formation and matrix continuity in SH system. Improved flexural strength indicates better crack control and greater suitability for structural elements like slabs, beams, pavements and so on.
3.4. SEM analysis
Microstructural Characteristics of 28 days samples were examined using SEM and the corresponding elemental composition was analysed using EDS elemental mapping and spot analysis at selected region in Backscattered Electron (BSE) mode to enhance contrast between unreacted particles and the surrounding gel. Figure 12 is the SEM image of SH mix and Figure 13 represents the elemental mapping graph of SH system. Figure 14 shows the EDS spectrum of the SH mix. The SEM image reveal a heterogeneous composite matrix that contains angular particles of precursors integrated in a continuous binder phase. The SH mix exhibited a comparatively compact geopolymer matrix with fewer microcracks and reduced pore distribution, indicating enhanced polymerisation and effective gel development at 28 days. The EDS spectrum highlights the presence of Sodium (Na), Aluminium (Al), Calcium (Ca) and Silicon (Si) in the hardened sample. The highest Na/Al ratio of the SH sample correlates with the highest compressive strength. The higher availability of sodium charge balances the aluminosilicate species and increase the network polymerization and reduces the defects producing denser gel network. The elemental composition is consistent with coexistence of N-A-S-H and C-A-S-H gel types reaction products reported in previous studies [26]. The minor peaks like iron (Fe) can be attributed to unreacted fly ash particles in SEM image which also less compared to other systems in this study. Thus, from the microstructural and elemental analysis, the co-occurrence of C-A-S-H and N-A-S-H gel may have contributed to improve matrix continuity and reduced pore structure, which is correlated with higher compressive strength observed in SH mixes.
SEM images of the SS sample shown in Figure 15 indicated a compact and well bonded matrix with minimal microcracks. The interfacial bond present was comparatively less compact than the SH mix. The elemental mapping is consistent with the coexistence of indicative C-A-S-H and N-A-S-H gel phases. These findings may be confirmed through EDS spectrum (Figures 16 and 17) where the presence of Sodium (Na) and Aluminium (Al) peaks represents the aluminosilicate (N-A-S-H) network and Calcium (Ca) and Silicon (Si) peaks represent the coexistence of C-A-S-H gel phase. The peaks of Iron (Fe) and other elements like magnesium (Mg) are relatively lower than that of SH mix which indicated better geopolymerization. Thus, geopolymerization kinetics greatly depend on the activator chemistry and the precursor composition [23]. But from the EDS analysis it can be found that the compressive strength does not depend on complete geopolymerization alone.
In contrast, the SC system (Figure 18) exhibited a relatively less dense microstructure with visible voids. Unreacted fly ash particles were observed with apparently low interfacial bonding. Also the Na/Al ratio is relatively lower than SS mix. This lower ratio indicates the minimum sodium availability for forming more connected N-A-S-H network making it less dense. From Figures 19 and 20 the presence of Fe and Mg peaks indicated the unreacted Fly ash particles ensuring incomplete geopolymerization. The occurrence of dominating C-A-S-H gel relative to N-A-S-H type gel phase was observed from the graph in Figure 19 and Table 11 compared to SH and SS mixes. This indicates that geopolymerization reaction was completely depended on GGBS reactivity rather than the alkalinity of sodium carbonate [14]. Thus, SC mix has lower compressive strength performance due to lack of sodium ions to densify the matrix though the geopolymerization was driven by GGBS.
From the Table 11 and the SEM-EDS analysis it is seen that Na/Al ratio and compressive strength followed the same trend whereas, the Ca/Si ratio does not follow the same trend indicating calcium incorporation alone is not the dominant strength controlling factor in One-part geopolymer systems and it may be concluded that it helped in early gel development and improved continuity alone. Instead the sodium availability for charge balance the aluminosilicate network is a key factor governing the strength. Finally, activator chemistry influence geopolymerization reaction, gel formation, pore distribution and sodium availability ensured matrix refinement, which collectively governed the mechanical performance of ambient cured One-part GPC systems [33].
3.5. XRD test
The XRD patterns of SH, SS and SC mix samples (Figure 21) indicate the coexistence of crystalline phases superimposed on the broad amorphous hump which is a characteristic of geopolymerization in alkali activated systems. The prominent peak observed around 26°–28.1° 2θ is attributed to crystalline phases of quartz and mullite, both of these are inherited from the residual fly ash. This is known to remain largely unreacted in ambient cured one-part geopolymer concrete because of their crystalline lattice is resistant to dissolution under mild alkaline environment. The minor peaks observed between 30°–55° 2θ are also associated with residual crystalline phases originating from the partially unreacted precursor materials [13]. Whereas, the low intensity peaks between 29°–30° 2θ tentatively represents calcite and may be associated with carbonation of calcium rich phases during geopolymerization. Minor calcite formation may contribute to partial pore refinement within the geopolymer matrix [33].
Comparison of the relative peak intensities among the three mixes revealed clear activator dependent differences. Among the three samples, SS mix exhibited the most intense and sharp crystalline peak at approximately 28.1° 2θ which is nearly double the times of the peak recorded by the SH mix and almost six times than that of SC mix. This indicates a comparatively higher residual fraction of unreacted crystalline precursor, possibly associated with incomplete dissolution of fly ash particles or residual sodium metasilicate. In contrast, the SC mix showed the lowest crystalline peak intensity and the broadest and most dominant amorphous hump, while SH showed crystalline peak with intermediate sharpness.
Notably this trend was not parallel to the mechanical strength because the SH mix with highest compressive strength (38.98 MPa) showed sharper crystalline peaks than the SC mix with lowest compressive strength (15.24 MPa). This indicates that the crystalline peak contribution between 26°–28.1° 2θ region is likely due to the inert quartz derived from the aggregate fraction rather than unreacted precursor and therefore does not directly reflect the efficiency of gel network formation.
This interpretation is thus supported by the EDS analysis, which revealed a significantly higher Na/Al atomic ratio for SH (0.79) than for SC (0.48), suggesting that more sodium is available in SH for charge balancing the aluminosilicate structure. Therefore, the gel network is more extensively cross linked in SH than in SC, despite the sharper XRD peaks. The findings indicate that the Na/Al ratio and the overall network connectivity are more reliable parameters to assess the quality of the gel and the mechanical properties of the ambient cured one-part geopolymer concrete system than the XRD amorphous fraction. This result highlights the need to use XRD in conjunction with other microstructural studies like SEM-EDS for understanding the geopolymerization behaviour, as the bulk phase composition may be misleading if there are contributions from inert crystalline aggregates.
4. DURABILITY AND COST COMPARISON
4.1. Durability analysis
To examine the long-term service behaviour of the one-part geopolymer concrete mixes, the SH and SS mixes were tested for acid resistance, sulphate resistance, water absorption, sorptivity and rapid and carbonation tests. These test results were compared with a conventional OPC control mix. The SC mix was excluded for durability study because while exposing the SC mix specimens to open air for a week after 28 days wrapped curing, they exhibited progressive surface deterioration, with distinct white powdery patches appearing on the cube surfaces as shown in Figure 22. This degradation intensified over time, ultimately resulting in loss of exposed surface layer of the cubes. This behaviour is consistent with efflorescence related deterioration previously reported in air cured, carbonate activated fly ash/slag geopolymer systems, where migration and surface carbonation of unreacted or excess alkali species progressively disrupts the near surface gel structure [40].
4.2. Acid resistance test
Acid resistance test is one of the severe durability tests in concrete as the acid solution progressively dissolve the binder, increase the pore connectivity and reduce the mechanical stability of the concrete. Therefore, evaluating acid resistance is essential for determining the long term durability of the OGPC in aggressive environment.
The acid resistance results in Figure 23 and Table 12 showed that both geopolymer concrete mixes had better resistance to weight loss under the acids than conventional OPC concrete. The SH mix showed a higher residual strength after exposure to Hydrochloric acid (HCl), as the well balanced aluminosilicate network prevented the penetration of HCl acid and reduced the weight loss. Similar behaviour has been reported for ambient cured OGPC where the chemically stable N-A-S-H gel and the lower calcium in the concrete significantly lower the mass loss and retained better strength compared to OPC, when exposed to acid attack [41, 42]. Similarly, geopolymer systems with less pore connectivity and finer microstructures have been demonstrated to be more resistant to aggressive ions in acidic conditions [43, 44].
Whereas, the SS mix was more resistant to Sulphuric acid (H2SO4) exposure than SH mix, suggesting that the relative acid resistance of the two activator systems is not consistent but depends on the acid species. Hydrochloric acid mainly dissolves the binder through decalcification and leaching of alkali ions, while sulphuric acid additionally promotes the formation of gypsum and other expansive products in calcium rich matrices. The overall deterioration was the highest for OPC specimens, as expected due to the higher susceptibility of calcium rich (C-S-H) hydration products to acid dissolution. Thus OGPC mixes can be better durable in acid environment than OPC due to their unique N-A-S-H gel type matrix. The damages of the specimens after exposing to chemicals are shown in Figures 24 and 25.
4.3. Sulphate resistance test
Concrete structures in the presence of sulphate bearing soils and groundwater or marine environments are subjected to sulphate attack. Sulphate ions penetrate the concrete matrix causing the development of expansive reaction products leading to cracks, loss of strength and deterioration of the binder. Thus, it is necessary to test the resistance to sulphates of one-part geopolymer concrete to determine the durability of the material in the presence of chemically aggressive environments.
When both geopolymer samples were exposed to 5% magnesium sulphate solution, it was found that both mixes had a significantly higher sulphate resistance than that of OPC and is represented in Figure 26, in terms of both weight loss and strength retention. Unlike OPC, where sulphate ions react with calcium hydroxide and hydrated calcium aluminates to form expansive gypsum and ettringite, the geopolymer binder contains a chemically stable N-A-S-H framework that significantly limits these deterioration mechanisms. Consequently, the lower weight loss and improved strength retention were observed in the present study. This indicates that the ingress of sulphate ions was effectively restricted, thereby minimizing internal expansion and microstructural damage. Similar behaviour has been reported for ambient cured one-part geopolymer systems, where geopolymer binders exhibited considerably higher sulphate resistance than OPC due to the absence of portlandite [42, 44]. In addition, it has been found in previous studies that a decrease in the pore connectivity and well refined geopolymer matrix can effectively prevent the penetration of sulphate ions and improve long-term durability under aggressive exposure conditions [41, 42]. The chemical stability of ambient cured one-part geopolymer concrete in sulphate rich environment is confirmed by the similar performance of SH and SS compared to OPC.
4.4. Water absorption and sorptivity test
Water absorption and sorptivity are important indicators of pore connectivity and permeability. The SH mix had the lowest values of both parameters given in Table 13, which suggested a dense and refined pore structure that was able to effectively limit the movement of capillary water, as the combined activation of NaOH-Na2SiO3 resulted in a more complete and compact gel network.
The values water absorption of the SS mix was slightly higher than SH mix, but were still lower than those of OPC concrete that had the highest water absorption and sorptivity, indicating that the microstructure of OGPC concrete was comparatively dense and less permeable. The lower water absorption and sorptivity values for the SH and SS mixes indicate that the water transport through the geopolymer matrix was significantly less than that of OPC concrete. The decreased capillary absorption indicates reduced pore interconnectivity resulting in reduced ingress of moisture and aggressive ions that cause deterioration in long run. Similar observations have been reported for ambient cured OGPC systems, where reduced water absorption was attributed to the formation of a compact aluminosilicate binder with lower permeability than conventional cement based materials [43].
The present results are consistent with the above findings where hybrid SH system exhibited lowest water absorption of 1.5%. Thus both SEM and water absorption test indicate that the occurrence of connected pore is very much less in OGPC with hybrid activators than OPC which reduce the transportation pathways for water making in more water resistant. The water absorption and Sorptivity of the samples are given in Figures 27 and 28.
4.5. Carbonation resistance test
Carbonation is major durability concern for reinforced concrete and is primarily governed by carbon dioxide (CO2) ingress, pore connectivity and binder chemistry. The carbonation depth is an indicator of concrete resistance to CO2 penetration and is closely related to the permeability and continuity of the hardened binder system.
The carbonation test results using phenolphthalein solution as shown in Figure 29 confirmed the comparatively denser microstructure of the SH mix, as it had the lowest carbonation depth indicated in Table 14, which meant that the SH mix had the highest resistance to CO2 ingress among all three mixes. The same behaviour has been observed for previous studies with same systems, with lower permeability and lower pore connectivity resulting in better resistance to CO2 ingress than conventional cement based materials [42, 44]. Previous studies have also demonstrated that the continuity of the geopolymer binder plays a more significant role in controlling carbonation than compressive strength alone, as the transport of carbon dioxide is primarily governed by the accessibility of interconnected pores [41]. The carbonation depth of the SS mix was higher than that of OPC, which is likely related to its lower calcium availability and slightly higher capillary porosity compared to SH. The results show that the carbonation resistance of the hybrid solid activation (SH) is better than the single-activator (SS) system in ambient curing.
4.6. Cost analysis
A material cost analysis was carried out on a per cubic metre basis of the developed one-part geopolymer concrete mixes and normalized by the 28-day compressive strength to evaluate the economic viability of the developed mixes in addition to their mechanical and durability performance.
The cost analysis of materials used in each mix was given in Table 15, was done for the materials used in this project alone with reference to material calculation Table 4. The findings showed that the cost efficiency per unit strength of the three geopolymer mixes was significantly different from the OPC control mix, despite the fact that all three mixes had a higher raw material cost per cubic metre, which is mainly due to the cost of solid alkaline activators. The absolute material cost of the SH mix is the highest among all the geopolymer mixes, but the cost performance ratio of the SH mix is noticeable among the other geopolymer mixes given in Table 16, which is only 14.4% higher than OPC. Though it is higher, the noticeable strength and durability performance of the SH mix helps it to be less maintained, keeping the life cycle cost lower. This distinction between initial material cost and life-cycle cost is a key consideration for practical adoption of OGPC in field applications and is consistent with broader life-cycle assessment findings reported for geopolymer systems in the literature [3, 4].
The SS mix, on the other hand, was slightly more expensive in absolute terms but had a satisfactory cost per unit strength because of its lower 28-day strength compared to its activator cost, suggesting that the sodium metasilicate system, although safer to handle, does not convert its activator cost into strength as effectively as the hybrid SH system. The poor cost-efficiency for the SC mix was observed due to its low compressive strength. The corresponding low Na/Al ratio found in the EDS analysis of SC mix reduced the sodium availability for charge balancing the aluminosilicate structure not only affected the mechanical performance but also made the activator cost economically unproductive. The subsequent surface deterioration of the SC mix under ambient curing negates any economic viability, regardless of the cost per MPa value of the mix at 28 days.
The cost analysis collectively suggests that the choice of activator for one-part geopolymer concrete should not be based solely on the cost of raw material, but should be based on a joint evaluation of the cost normalized by strength and durability performance. Based on this, the hybrid activator system (SH) which combines sodium hydroxide and sodium metasilicate is the most economical among the systems studied, having the best initial cost, mechanical performance and life-cycle economy due to durability, while the SC system in its current composition and curing method is not recommended for structural application.
5. CONCLUSION
The experimental results demonstrated that hybrid solid activator systems significantly influence geopolymerization behaviour, matrix development, mechanical and durability performance of ambient cured one-part geopolymer concrete. Among the systems investigated, the hybrid sodium hydroxide-sodium metasilicate activated system achieved the highest compressive strength of about 39 MPa at 28 days, which is 37% higher compared to that of Ordinary Portland cement concrete under similar curing conditions. The Sodium metasilicate activated system showed moderate strength development and improved handling characteristics, indicating their potential as a safer alternative for practical applications. In contrast, sodium carbonate activated mixes exhibited delayed reaction kinetics and lower strength development, primarily due to slower geopolymerization with lower alkalinity and delayed precursor dissolution. Further, this system exhibited progressive surface efflorescence and structural disintegration under prolonged ambient curing, clarifying that it is unsuitable for durability evaluation and practical structural application in its current formulation. SEM-EDS and XRD analysis confirmed that improved mechanical performance was associated with improved microstructure driven by the sodium availability for charge balance the aluminosilicate network, reduced pore structure and the co-occurrence of N-A-S-H and C-A-S-H gel phases. These findings establish the critical role of solid activator in controlling geopolymerization mechanisms, phase evolution and strength development in ambient cured one-part geopolymer concrete.
Overall, the study demonstrates that optimized hybrid solid activator systems particularly the SH system can achieve the strength and durability performance with the potential for structural applications under ambient curing. It also ensures mechanical performance comparable to conventional Two-part geopolymer systems in addition to improved safety and field applicability. The findings provide grounds for future investigations focusing on long term durability performance of SC system under modified curing regime, shrinkage behaviour and large-scale field applicability of ambient cured one-part GPC systems.
6. DATA AVAILABILITY
The entire dataset supporting the results of this study was published in the article itself.
7. BIBLIOGRAPHY
-
[1] SABĂU, M., BOMPA, D.V., SILVA, L.F.O., “Comparative carbon emission assessments of recycled and natural aggregate concrete: environmental influence of cement content”, Geoscience Frontiers, v. 12, n. 6, pp. 101235, Nov. 2021. doi: https://doi.org/10.1016/j.gsf.2021.101235.
» https://doi.org/10.1016/j.gsf.2021.101235 -
[2] SINGH, R.P., VANAPALLI, K.R., CHEELA, V.R.S., et al, “Fly ash, GGBS, and silica fume based geopolymer concrete with recycled aggregates: properties and environmental impacts”, Construction & Building Materials, v. 378, pp. 131168, May. 2023. doi: https://doi.org/10.1016/j.conbuildmat.2023.131168.
» https://doi.org/10.1016/j.conbuildmat.2023.131168 -
[3] BHAGATH SINGH, G.V.P., DURGA PRASAD, V., “Environmental impact of concrete containing high volume fly ash and ground granulated blast furnace slag”, Journal of Cleaner Production, v. 448, pp. 141729, Apr. 2024. doi: https://doi.org/10.1016/j.jclepro.2024.141729.
» https://doi.org/10.1016/j.jclepro.2024.141729 -
[4] FURTOS, G., PRODAN, D., SAROSI, C., et al, “The precursors used for developing geopolymer composites for circular economy—a review”, Materials (Basel), v. 17, n. 7, pp. 1696, Jan. 2024. doi: https://doi.org/10.3390/ma17071696. PMid:38612210.
» https://doi.org/10.3390/ma17071696 -
[5] RAJA, M.A., SUJATHA, S.J., “Geopolymer concrete cured under ambient conditions using a single alkali activator”, Matéria (Rio de Janeiro), v. 29, n. 3, pp. e20240281, 2024. doi: https://doi.org/10.1590/1517-7076-rmat-2024-0281.
» https://doi.org/10.1590/1517-7076-rmat-2024-0281 -
[6] GUO, Y., CHEN, S., LAKHIAR, M.T., et al, “Ternary binders and recycled turbine blade fibres in mortar: Reducing embodied carbon in coastal construction”, Construction & Building Materials, v. 501, pp. 144277, Nov. 2025. doi: https://doi.org/10.1016/j.conbuildmat.2025.144277.
» https://doi.org/10.1016/j.conbuildmat.2025.144277 -
[7] AZAD, N.M., SAMARAKOON, S.M.S.M.K., “Utilization of industrial by-products/waste to manufacture geopolymer cement/concrete”, Sustainability (Basel), v. 13, n. 2, pp. 873, Jan. 2021. doi: https://doi.org/10.3390/su13020873.
» https://doi.org/10.3390/su13020873 -
[8] JAHANDARI, S., TAO, Z., RAHMANI, A., et al, “Durability of one-part geopolymer concrete in aggressive environments”, Construction & Building Materials, v. 490, pp. 142510, Sep. 2025. doi: https://doi.org/10.1016/j.conbuildmat.2025.142510.
» https://doi.org/10.1016/j.conbuildmat.2025.142510 -
[9] SONG, Y., DIAO, X., XU, R., et al, “A comprehensive review of mineral carbonation of civil engineering materials: a bibliometric analysis”, Environmental Science & Technology, v. 59, n. 50, pp. 26917–26944. doi: https://doi.org/10.1021/acs.est.5c03561.
» https://doi.org/10.1021/acs.est.5c03561 -
[10] DONG, M., ELCHALAKANI, M., KARRECH, A., “Development of high strength one-part geopolymer mortar using sodium metasilicate”, Construction & Building Materials, v. 236, pp. 117611, Mar. 2020. doi: https://doi.org/10.1016/j.conbuildmat.2019.117611.
» https://doi.org/10.1016/j.conbuildmat.2019.117611 -
[11] MAHMOOD, A.H., FOSTER, S.J., CASTEL, A., “Effects of mixing duration on engineering properties of geopolymer concrete”, Construction & Building Materials, v. 303, pp. 124449, Oct. 2021. doi: https://doi.org/10.1016/j.conbuildmat.2021.124449.
» https://doi.org/10.1016/j.conbuildmat.2021.124449 -
[12] NISHANTH, L., PATIL, D.N.N., “Experimental evaluation on workability and strength characteristics of self-consolidating geopolymer concrete based on GGBFS, flyash and alccofine”, Materials Today: Proceedings, v. 59, pp. 51–57, Jan. 2022. doi: https://doi.org/10.1016/j.matpr.2021.10.200.
» https://doi.org/10.1016/j.matpr.2021.10.200 -
[13] LENIN, S., ROSELIN, R., “Fresh properties and strength characteristics of ambient geopolymer concrete with ground granulated blast furnace slag”, Matéria (Rio de Janerio), v. 30, p. e20240795, 2025, doi: https://doi.org/10.1590/1517-7076-RMAT-2024-0795.
» https://doi.org/10.1590/1517-7076-RMAT-2024-0795 -
[14] LAO, J.-C., XU, L.-Y., HUANG, B.-T., et al, “Utilization of sodium carbonate activator in strain-hardening ultra-high-performance geopolymer concrete (SH-UHPGC)”, Frontiers in Materials, v. 10, pp. 1142237, Feb. 2023. doi: https://doi.org/10.3389/fmats.2023.1142237.
» https://doi.org/10.3389/fmats.2023.1142237 -
[15] MESHRAM, R.B., KUMAR, S., “Comparative life cycle assessment (LCA) of geopolymer cement manufacturing with Portland cement in Indian context”, International Journal of Environmental Science and Technology, v. 19, n. 6, pp. 4791–4802, Jun. 2022. doi: https://doi.org/10.1007/s13762-021-03336-9.
» https://doi.org/10.1007/s13762-021-03336-9 -
[16] WAN-EN, O., YUN-MING, L., CHENG-YONG, H., et al, “Towards greener one-part geopolymers through solid sodium activators modification”, Journal of Cleaner Production, v. 378, pp. 134370, Dec. 2022. doi: https://doi.org/10.1016/j.jclepro.2022.134370.
» https://doi.org/10.1016/j.jclepro.2022.134370 -
[17] KERR, J., RAYBURG, S., NEAVE, M., et al, “Comparative Analysis of the Global Warming Potential (GWP) of structural stone, concrete and steel construction materials”, Sustainability (Basel), v. 14, n. 15, pp. 9019, Jan. 2022. doi: https://doi.org/10.3390/su14159019.
» https://doi.org/10.3390/su14159019 -
[18] WAN, F., GUO, Y., ZHUANG, S., et al, “Towards practical application of eco-friendly engineered geopolymer composites: achieving strength-ductility synergy through low fibre volume design”, Journal of Building Engineering, v. 113, pp. 114171, Nov. 2025. doi: https://doi.org/10.1016/j.jobe.2025.114171.
» https://doi.org/10.1016/j.jobe.2025.114171 -
[19] REDDY, K.C., SUBRAMANIAM, K.V.L., “Investigation on the roles of solution-based alkali and silica in activated low-calcium fly ash and slag blends”, Cement and Concrete Composites, v. 123, pp. 104175, Oct. 2021. doi: https://doi.org/10.1016/j.cemconcomp.2021.104175.
» https://doi.org/10.1016/j.cemconcomp.2021.104175 -
[20] SHAMSAH, M., KALFAT, R., SUBRAMANIAM, K.V.L., et al, “Calcium enhanced ambient cured fly Ash based geopolymer binders”, Scientific Reports, v. 15, n. 1, pp. 25603, Jul. 2025. doi: https://doi.org/10.1038/s41598-025-07854-1. PMid:40664745.
» https://doi.org/10.1038/s41598-025-07854-1 -
[21] LI, Y., DONG, Y., EL-NAGGAR, M.R., et al, “The influence of particle size and calcium content on performance characteristics of metakaolin- and fly-ash-based geopolymer gels”, Gels (Basel, Switzerland), v. 10, n. 10, pp. 639, Oct. 2024. doi: https://doi.org/10.3390/gels10100639. PMid:39451292.
» https://doi.org/10.3390/gels10100639 -
[22] ANBARASU, N.A., SIVAKUMAR, V., YUVARAJ, S., et al, “Pioneering the next frontier in construction with high-strength concrete infused by nano materials”, Matéria (Rio de Janerio), v. 30, p. e20240730, 2025, doi: https://doi.org/10.1590/1517-7076-rmat-2024-0730.
» https://doi.org/10.1590/1517-7076-rmat-2024-0730 -
[23] NAGAJOTHI, S., ELAVENIL, S., “Effect of GGBS addition on reactivity and microstructure properties of ambient cured fly ash based geopolymer concrete”, Silicon, n. 13, pp. 507-516, 2021. doi: https://doi.org/10.1007/s12633-020-00470-w.
» https://doi.org/10.1007/s12633-020-00470-w -
[24] YILMAZOGLU, A., YILDIRIM, S.T., YILDIZ, S., et al, “Effect of GGBS content and water/geopolymer solid ratio on the mechanical, elevated temperature resistance, and sorptivity properties of fa/ggbs-based geopolymer concrete”, Journal of Materials in Civil Engineering, v. 36, n. 4, pp. 04024032, Apr. 2024. doi: https://doi.org/10.1061/JMCEE7.MTENG-17167.
» https://doi.org/10.1061/JMCEE7.MTENG-17167 -
[25] WU, X., SHEN, Y., HU, L., “Performance of geopolymer concrete activated by sodium silicate and silica fume activator”, Case Studies in Construction Materials, v. 17, pp. e01513, Dec. 2022. doi: https://doi.org/10.1016/j.cscm.2022.e01513.
» https://doi.org/10.1016/j.cscm.2022.e01513 -
[26] LIVI, C.N., Repette, W.L. “Effect of NaOH concentration and curing regime on geopolymer”, Revista IBRACON Structures and Materials Journal, v. 10, n. 6, pp. 1174–1181, Nov.2017, doi: https://doi.org/10.1590/s1983-41952017000600003.
» https://doi.org/10.1590/s1983-41952017000600003 -
[27] LI, C., ZHANG, X., SHI, T., et al, “Enhancement of the mechanical properties and spatial uniformity of lightweight expanded polystyrene concrete using carbonated recycled fine aggregate”, Case Studies in Construction Materials, v. 24, pp. e05864, Jul. 2026. doi: https://doi.org/10.1016/j.cscm.2026.e05864.
» https://doi.org/10.1016/j.cscm.2026.e05864 - [28] YUVARAJ, K., SAKTHIVEL, M., KARTHICK, M.D., et al, “Mechanical performance of mono and hybrid synthetic fibers engineered cementitious composites with silica fume”, Journal of Ceramic Processing Research, v. 25, n. 2, pp. 254–260, Apr. 2024.
-
[29] KANDASWAMY, S., SHANMUGAM, B., MUNUSWAMY, M.G., et al, “A comprehensive study on microbial self-healing concrete for sustainable construction”, Matéria (Rio de Janerio), v. 29, p. e20240181, 2024, doi: https://doi.org/10.1590/1517-7076-RMAT-2024-0181.
» https://doi.org/10.1590/1517-7076-RMAT-2024-0181 -
[30] SRINIVASAN, R., DEEPALAKSHMI, R., BASKARAN, J., et al, “Investigation on the mechanical properties of micro-sized B4C particles reinforced with FSW of aluminium alloy composites”, Materials Today: Proceedings, n. Jun, 2023. doi: https://doi.org/10.1016/j.matpr.2023.05.476.
» https://doi.org/10.1016/j.matpr.2023.05.476 - [31] BUREAU OF INDIAN STANDARDS, IS 516:1959 Method of Tests for Strength of Concrete, New Delhi, Bureau of Indian Standards, 1959.
- [32] BUREAU OF INDIAN STANDARDS, IS 5816:1999,Splitting Tensile Strength of Concrete – Method of Test, New Delhi, Bureau of Indian Standards, 1999.
-
[33] HASSAN, A., ARIF, M., SHARIQ, M., “Influence of microstructure of geopolymer concrete on its mechanical properties—a review”, In: Shukla, S.K., Barai, S.V., Mehta, A. (Eds.), Advances in Sustainable Construction Materials and Geotechnical Engineering, Singapore: Springer, pp. 119–129, 2020. doi: https://doi.org/10.1007/978-981-13-7480-7_10.
» https://doi.org/10.1007/978-981-13-7480-7_10 -
[34] ZENG, H., JIN, M., LI, W., et al, “Thermal-fatigue challenges in the interfacial transition zone (ITZ) of concrete: How fly ash modulates degradation?”, Cement and Concrete Composites, v. 168, pp. 106500, Apr. 2026. doi: https://doi.org/10.1016/j.cemconcomp.2026.106500.
» https://doi.org/10.1016/j.cemconcomp.2026.106500 -
[35] HOMBALI, A., SELVAM, J., “Performance evaluation of low-carbon geopolymer concrete incorporating industrial and agricultural wastes”, Matéria (Rio de Janerio), v. 30, p. e20250723, 2025, doi: https://doi.org/10.1590/1517-7076-RMAT-2025-0723.
» https://doi.org/10.1590/1517-7076-RMAT-2025-0723 -
[36] SAJAN, P., JIANG, T., LAU, C., et al, “Combined effect of curing temperature, curing period and alkaline concentration on the mechanical properties of fly ash-based geopolymer”, Cleaner Materials, v. 1, pp. 100002, Dec. 2021. doi: https://doi.org/10.1016/j.clema.2021.100002.
» https://doi.org/10.1016/j.clema.2021.100002 - [37] BUREAU OF INDIAN STANDARDS, IS 4031-5 Methods of physical tests for hydraulic cement, Part 5: Determination of initial and final setting times, New Delhi, Bureau of Indian Standards, 1988
- [38] BUREAU OF INDIAN STANDARDS, IS 1199: Part 6:2018Fresh Concrete — Methods of Sampling, Testing and Analysis Part 6 Tests on Fresh Self Compacting Concrete (First Revision), New Delhi, Bureau of Indian Standards, 2018.
-
[39] HASSAN, A., ALOMAYRI, T., NOAMAN, M.F., et al, “3D printed concrete for sustainable construction: a review of mechanical properties and environmental impact”, Archives of Computational Methods in Engineering, v. 32, n. 5, pp. 2713–2743, Jun. 2025. doi: https://doi.org/10.1007/s11831-024-10220-5.
» https://doi.org/10.1007/s11831-024-10220-5 -
[40] NAGHIZADEH, A., TCHADJIE, L., SOLOMON, F., et al, “Efflorescence and strength effects of different ambient regimes of curing fly ash – based geopolymer concrete”, Construction & Building Materials, v. 516, pp. 145722, Mar. 2026. doi: https://doi.org/10.1016/j.conbuildmat.2026.145722.
» https://doi.org/10.1016/j.conbuildmat.2026.145722 -
[41] JAHANDARI, S., TAO, Z., RAHMANI, A., et al, “Durability of one-part geopolymer concrete in aggressive environments”, Construction & Building Materials, v. 490, pp. 142510, Sep. 2025. doi: https://doi.org/10.1016/j.conbuildmat.2025.142510.
» https://doi.org/10.1016/j.conbuildmat.2025.142510 -
[42] ERYILMAZ, K., POLAT, R., “Sustainable concrete production: mechanical and durability behaviour of slag-based geopolymer containing recycled geopolymer aggregate”, Journal of Building Engineering, v. 96, pp. 110512, Nov. 2024. doi: https://doi.org/10.1016/j.jobe.2024.110512.
» https://doi.org/10.1016/j.jobe.2024.110512 -
[43] GERALDO, R.H., GONÇALVES, J.P., CAMARINI, G., “Durability of one-part alkali-activated binder made with alternative sodium silicate”, Construction Materials, v. 6, n. 1, pp. 8, Jan. 2026. doi: https://doi.org/10.3390/constrmater6010008.
» https://doi.org/10.3390/constrmater6010008 -
[44] RAJALEKSHMI, P., JOSE, P.A., “Influence of eco-friendly lightweight aggregates in mechanical and durability properties of geopolymer concrete”, Matéria (Rio de Janerio), v. 28, n. 4, p. e20230209, 2023. doi: https://doi.org/10.1590/1517-7076-RMAT-2023-0209.
» https://doi.org/10.1590/1517-7076-RMAT-2023-0209